MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Magnesium
Magnesium Elektron - Service & Innovation in Magnesium

Magnesium Elektron Elektron® AZ91 Magnesium Alloy
Categories: Metal; Nonferrous Metal; Magnesium Alloy

Material Notes: General purpose alloy. Good founding properties. Suitable for pressure die castings.

Information provided by Magnesium Elektron.

Vendors: Magnesium Elektron is the world leader in high strength magnesium alloys in rolled, extruded and cast forms. Phone (303) 589-3189 or visit www.magnesium-elektron.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.83 g/cc1.83 g/cc
 
Mechanical PropertiesMetricEnglishComments
Hardness, Vickers 60 - 7560 - 75as sand cast
 60 - 7560 - 75sand cast + solution treated
 85 - 10085 - 100sand cast + solution and precipitation treated
Tensile Strength at Break 125 MPa18100 psiSand cast
 170 MPa24700 psiChill cast
 200 MPa29000 psiSand cast, + solution treated
 200 MPa29000 psiSand cast, solution treated and precipitation treated
 215 MPa31200 psiChill cast, + solution treated
 215 MPa31200 psiChill cast, solution and precipitation treated
Tensile Strength, Yield  80.0 MPa
@Strain 0.2 %
11600 psi
@Strain 0.2 %
solution treated
 95.0 MPa
@Strain 0.2 %
13800 psi
@Strain 0.2 %
Sand cast
 100 MPa
@Strain 0.2 %
14500 psi
@Strain 0.2 %
Chill cast
 120 MPa
@Strain 0.2 %
17400 psi
@Strain 0.2 %
solution and precipitation treated
Elongation at Break 2.0 %2.0 %
 2.0 %2.0 %Chill cast
 4.0 %4.0 %Chill cast, + solution treated
 4.0 %4.0 %Sand cast, + solution treated
 5.0 %5.0 %Chill cast, solution and precipitation treated
Compressive Yield Strength  75.0 - 110 MPa
@Strain 0.2 %
10900 - 16000 psi
@Strain 0.2 %
solution and precipitation treated
 85.0 - 110 MPa
@Strain 0.2 %
12300 - 16000 psi
@Strain 0.2 %
as cast
 110 - 140 MPa
@Strain 0.2 %
16000 - 20300 psi
@Strain 0.2 %
solution and precipitation treated
Compressive Strength 185 - 432 MPa26800 - 62700 psiSolution treated
 280 - 340 MPa40600 - 49300 psias cast
 385 - 465 MPa55800 - 67400 psisolution and precipitation treated
Fatigue Strength  58.0 - 62.0 MPa
@# of Cycles 5.00e+7
8410 - 8990 psi
@# of Cycles 5.00e+7
Rotating bend; semi-circular notch, radius 1.2 mm, solution and precipitation treated
 58.0 - 65.0 MPa
@# of Cycles 5.00e+7
8410 - 9430 psi
@# of Cycles 5.00e+7
Rotating bend; semi-circular notch, radius 1.2 mm, as cast
 65.0 - 77.0 MPa
@# of Cycles 5.00e+7
9430 - 11200 psi
@# of Cycles 5.00e+7
Rotating bend; semi-circular notch, radius 1.2 mm, solution treated
 70.0 - 77.0 MPa
@# of Cycles 5.00e+7
10200 - 11200 psi
@# of Cycles 5.00e+7
Unnotched Rotating Bend, solution and precipitation treated
 75.0 - 85.0 MPa
@# of Cycles 5.00e+7
10900 - 12300 psi
@# of Cycles 5.00e+7
Unnotched Rotating Bend, as cast
 77.0 - 92.0 MPa
@# of Cycles 5.00e+7
11200 - 13300 psi
@# of Cycles 5.00e+7
Unnotched Rotating Bend, solution treated
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000141 ohm-cm0.0000141 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 27.0 µm/m-°C
@Temperature 20.0 - 200 °C
15.0 µin/in-°F
@Temperature 68.0 - 392 °F
Specific Heat Capacity 1.00 J/g-°C0.239 BTU/lb-°F
Thermal Conductivity 84.0 W/m-K583 BTU-in/hr-ft²-°F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 9.5 %9.5 %
Magnesium, Mg 89.7 %89.7 %As Balance
Manganese, Mn 0.30 %0.30 %
Zinc, Zn 0.50 %0.50 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
SAE AZ91 Magnesium Matrix Composite, as cast
SAE SiC/AZ91 Magnesium Matrix Composite, as cast
Magnesium WE43-T6, Cast
Magnesium Elektron Elektron® AZ31B Magnesium Extrusion Alloy, UNS M11311
Magnesium AZ91D-F, Cast

NMAGEL940 / 186955

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.