MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

3M Dyneon™ 81T High Temperature Perfluoroelastomer
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes: 3M™ Dyneon™ PFE 81TZ is a technically advanced high temperature perfluoroelastomer (HT PFE). It is designed to meet the challenges of higher temperature applications. It is classified as FFKM per ASTM D1418. Its fully fluorinated back bone structure provides a very broad chemical and thermal stability

    Features and Benefits:
  • Ideal for dry side (thermal processes) semiconductor applications including plasma, and high temperature CPI and aerospace applications High temperature FFKM
  • Low metal ion content with low extractables
  • Upper use temperature of 315°C
  • Good compression set resistance
  • Can be compounded to pass AMS 7257C
  • Can be used to blend with other High Temperature FFKM to adjust ultimate elongation, lower Durometer, and allow for a higher percent deformation of seals in us

Information provided by the Dyneon division of 3M.

Key Words: Formerly 81TZ
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 2.00 g/cc2.00 g/cc
Mooney Viscosity 80
@Temperature 121 °C
80
@Temperature 250 °F
ML 1+10
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 7171Press cure 15 Minutes @ 188°C, Post Cure 24 Hours @ 250°C; ASTM D2240
Tensile Strength at Break 11.9 MPa1730 psiPress cure 15 Minutes @ 188°C, Post Cure 24 Hours @ 250°C
Elongation at Break 230 %230 %Press cure 15 Minutes @ 188°C, Post Cure 24 Hours @ 250°C
100% Modulus 4.70 MPa
@Strain 100 %
682 psi
@Strain 100 %
Press cure 15 Minutes @ 188°C, Post Cure 24 Hours @ 250°C
Compression Set  27 %
@Treatment Temp. 232 °C,
Time 252000 sec
27 %
@Treatment Temp. 450 °F,
Time 70.0 hour
Method B, -214 O-rings, Aged 70 Hours, 25% Deformation; ASTM D395
 35 %
@Treatment Temp. 232 °C,
Time 605000 sec
35 %
@Treatment Temp. 450 °F,
Time 168 hour
Method B, -214 O-rings, Aged 168 Hours, 25% Deformation; ASTM D395
 50 %
@Treatment Temp. 300 °C,
Time 252000 sec
50 %
@Treatment Temp. 572 °F,
Time 70.0 hour
Method B, -214 O-rings, Aged 70 Hours, 18% Deformation; ASTM D395
 61 %
@Treatment Temp. 300 °C,
Time 605000 sec
61 %
@Treatment Temp. 572 °F,
Time 168 hour
Method B, -214 O-rings, Aged 168 Hours, 18% Deformation; ASTM D395
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 315 °C599 °F
Brittleness Temperature -35.0 °C-31.0 °F
Transformation Temperature -2.00 °C28.4 °FTR10
 
Descriptive Properties
ColorWhite
FormCrumb
MH, Maximum Toque10.1 inch-lb100 cpm, 0.5° Arc, 6 Minutes @ 177°C
ML, Minimum Torque0.9 inch-lb100 cpm, 0.5° Arc, 6 Minutes @ 177°C
t2, Time to 2 Inch-lb Rise from Minimum3.4 Minute100 cpm, 0.5° Arc, 6 Minutes @ 177°C
t'50, Time to 50% Cure4.7 Minutes100 cpm, 0.5° Arc, 6 Minutes @ 177°C
t'90, Time to 90% Cure8.4 Minutes100 cpm, 0.5° Arc, 6 Minutes @ 177°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
3M Dyneon™ PFE 60 Perfluoroelastomer
3M Dyneon™ PFE 4131TZ High Temperature Perfluoroelastomer
3M Dyneon™ TFE 90 Peroxide Cure Perfluoroelastomer
DuPont Mobility and Materials Kalrez® 8002 FFKM Perfluoroelastomer
DuPont Mobility and Materials Kalrez® 8475 FFKM Perfluoroelastomer

PDYL9970 / 129988

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.