MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Chemours Viton® GF-600S with 30-MT Black Fluoroelastomer Compound
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes:
  • Cures exceptionally fast to a high state of cure
  • Exhibits improved mold release/mold fouling properties compared to Viton® GF
  • Exhibits improved mold flow, less shear sensitivity, and lower extruder die swell for a ~65 Mooney FKM
  • Exhibits excellent physical properties with high elongation, both original and aged
  • Exhibits similar heat, fluids, and low temperature resistance compared to Viton® GF
  • Exhibits excellent compression set resistance with short (2 hr) or no postcure

Chemours was formed from former DuPont performance chemicals businesses, including the Viton product line, in 2015.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 7070No Postcure; ASTM D2240
 77772 hours Postcure; ASTM D2240
Tensile Strength at Break 10.7 MPa1550 psiNo Postcure; ASTM D412
 18.3 MPa2650 psi2 hours Postcure; ASTM D412
Tensile Stress at Strain  0.700 MPa
@Strain 10 %
102 psi
@Strain 10 %
No Postcure; ASTM D412
 1.00 MPa
@Strain 10 %
145 psi
@Strain 10 %
2 hours Postcure; ASTM D412
Elongation at Break 302 %302 %2 hours Postcure; ASTM D412
 350 %350 %No Postcure; ASTM D412
100% Modulus  3.40 MPa
@Strain 100 %
493 psi
@Strain 100 %
No Postcure; ASTM D412
 5.40 MPa
@Strain 100 %
783 psi
@Strain 100 %
2 hours Postcure; ASTM D412
Compression Set  29 %
@Temperature 200 °C,
Time 79200 sec
29 %
@Temperature 392 °F,
Time 22.0 hour
O-Rings 2 hours postcure; ASTM D1414
 37 %
@Temperature 200 °C,
Time 79200 sec
37 %
@Temperature 392 °F,
Time 22.0 hour
O-Rings, no postcure; ASTM D1414
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -42.0 °C-43.6 °FPostcured
 -26.0 °C-14.8 °FNo Postcure
 
Processing PropertiesMetricEnglishComments
Processing Temperature  177 °C
@Time 299 sec
351 °F
@Time 0.0830 hour
Cure
 232 °C
@Time 7200 sec
450 °F
@Time 2.00 hour
Postcure
 
Component Elements PropertiesMetricEnglishComments
Fluorine, F 70 %70 %Uncompounded Viton
 
Descriptive Properties
Formulation as Tested0.5Armeen® 18D
 100GF-600S
 3Diak 7 (TAIC)
 3Varox® DBPH-50
 30MT Black

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
DuPont Mobility and Materials Hypalon® 45 Chlorosulfonated Polyethylene Rubber, Peroxide Cured Carbon Black Filled Compound
ATI Allvac® Vasco® 17-4 Precipitation Hardening Steel, Heat Treatment: 1038°C (1900°F) + Age
Chemours Viton® GBLT-600S Fluoroelastomer Compound
DuPont Mobility and Materials Kalrez® 4079 FFKM Perfluoroelastomer
DuPont Mobility and Materials Hypalon® 45 Chlorosulfonated Polyethylene Rubber, Carbon Black Filled Compound

PDVC9829 / 170470

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.