MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Aluminum Bronze, UNS C95400, Copper Casting Alloy, TQ50 Temper
Categories: Metal; Nonferrous Metal; Copper Alloy; Bronze; Copper Casting Alloy

Material Notes: Good wear resistance, heat treatable. Except where noted, all property values are for sand casting.

Recommended Casting Methods: Centrifugal, Continuous, Permanent Mold, Plaster, and Sand.

Applications:Pump impellers, bearings, gears, worms, bushings, valve seats and guides, rolling mill slippers, slides, nonsparking hardware.

Classified under: Aluminum bronzes. ASTM B148; formerly ASTM B148-9C

Key Words: Aluminum bronze, ASTM B148, ASTM B148-9C, CDA 954
Vendors: Dura-Bar Metal Services is a major distributor of bronze alloys. We stock a large inventory of C95400 in tubes, rounds and rectangles. Our customers rely on us for high quality materials that help increase their profitability. Call us at 1-800-526-0548 or visit dura-barms.com for more information.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 7.45 g/cc0.269 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 1951953000 kg
Hardness, Rockwell B 9494
Tensile Strength, Ultimate 620 MPa89900 psi
Tensile Strength, Yield 310 MPa45000 psi
Elongation at Break 8.0 %8.0 %in 50 mm
Reduction of Area 6.0 %6.0 %
Modulus of Elasticity 110 GPa16000 ksi
Compressive Strength 1070 MPa155000 psi
Poissons Ratio 0.3160.316
Fatigue Strength 240 MPa
@# of Cycles 1.00e+8
34800 psi
@# of Cycles 1.00e+8
Reverse Bending
Machinability 60 %60 %UNS C36000 (free-cutting brass) = 100%
Shear Modulus 41.0 GPa5950 ksi
Izod Impact 15.0 J11.1 ft-lb
Charpy Impact 9.00 J6.64 ft-lbKeyhole
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000133 ohm-cm
@Temperature 20.0 °C
0.0000133 ohm-cm
@Temperature 68.0 °F
Magnetic Permeability 1.21.216 kA/m field strength
 
Thermal PropertiesMetricEnglishComments
CTE, linear 16.2 µm/m-°C
@Temperature 20.0 - 300 °C
9.00 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.420 J/g-°C0.100 BTU/lb-°F
Thermal Conductivity 59.0 W/m-K
@Temperature 20.0 °C
409 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
Melting Point 1025 - 1040 °C1877 - 1900 °F
Solidus 1025 °C1877 °F
Liquidus 1040 °C1900 °F
Shrinkage 1.6 %1.6 %Patternmaker's Shrinkage (3/16 in./ft.)
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 620 °C1150 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 10 - 11.5 %10 - 11.5 %
Copper, Cu >= 83 %>= 83 %
Iron, Fe 3.0 - 5.0 %3.0 - 5.0 %
Manganese, Mn <= 0.50 %<= 0.50 %
Nickel, Ni <= 2.5 %<= 2.5 %includes Co
Other, total <= 0.50 %<= 0.50 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum Bronze, UNS C95400, Copper Casting Alloy, As Cast
High-Leaded Tin Bronze, UNS C93200, Copper Casting Alloy, Bearing Bronze SAE 660
Nickel Aluminum Bronze, UNS C63000, Annealed Rod
MetalTek MTEK 175-C Cast UNS C95400HT Aluminum Bronze
Oilite® Bronze Bearing Alloy - SAE 841

MC95400b2 / 171653

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.