MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

CeramTec 950 Zirconia Toughened Alumina (ZTA), Al2O3•ZrO2
Categories: Ceramic; Oxide; Aluminum Oxide

Material Notes: 950 has a combination of high strength (from zirconia) and high hardness (from the alumina phase). It has excellent wear resistance, both in sliding and abrasive conditions. This material offers a good compromise between toughened zirconia and alumina. It is a good choice for applications that require higher strength but lower hardness compared with alumina (e.g., textile wear parts). Produced with total dispersion of the zirconia phase in the alumina phase, 950 offers consistent performance, lot to lot.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 4.40 g/cc0.159 lb/in³DIN EN 623-2 / ASTM-C373 / ASTM-C20
Water Absorption 0.00 %0.00 %DIN EN 623-2 / ASTM-C373
 
Mechanical PropertiesMetricEnglishComments
Vickers Microhardness 15001500HV 0.5; DINV ENV 843-4
Tensile Strength at Break 414 MPa60000 psiACMA Test #4 / DIN EN 843-1
Tensile Modulus 289 GPa41900 ksiYoung's; DINV ENV 843-2 / ASTM-F417
Flexural Strength 680 MPa98600 psi20 x 40 mm
Compressive Strength 2890 MPa419000 psiASTM C-773-88 / DIN 51067T1
Poissons Ratio 0.220.22DINV ENV 843-2
Fracture Toughness 6.00 MPa-m½5.46 ksi-in½DIN 51109
Shear Modulus 126 GPa18300 ksi
 
Thermal PropertiesMetricEnglishComments
CTE, linear 8.80 µm/m-°C4.89 µin/in-°FDIN EN 821-1
 6.90 µm/m-°C
@Temperature 20.0 - 200 °C
3.83 µin/in-°F
@Temperature 68.0 - 392 °F
 7.80 µm/m-°C
@Temperature 20.0 - 600 °C
4.33 µin/in-°F
@Temperature 68.0 - 1110 °F
ASTM-C373
 8.30 µm/m-°C
@Temperature 20.0 - 1000 °C
4.61 µin/in-°F
@Temperature 68.0 - 1830 °F
Specific Heat Capacity 0.600 J/g-°C
@Temperature 100 - 200 °C
0.143 BTU/lb-°F
@Temperature 212 - 392 °F
DINV ENV 821-3
Thermal Conductivity 15.0 W/m-K104 BTU-in/hr-ft²-°FDIN EN 821-2 / ASTM-C408
Maximum Service Temperature, Air 1500 °C2730 °F
 
Descriptive Properties
ColorBuff
Te Value (°C)> 1000
Thermal Shock Resistance R1 (K)250Hasselman (Experimental)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
CeramTec 977 Zirconia Toughened Alumina (ZTA), Al2O3•ZrO2
CeramTec ATZ Alumina Toughened Zirconia, Dental Grade
CeramTec MZ BE Zirconia 3Y-TZP, Dental Grade
Kennametal Stellite Stellite® 21
Astro Met ZTA 96 Zirconia Toughened Alumina

CCERA936 / 107536

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.