Polyram Polytron A50B01 Nylon 6.6, 50% Long Fiber Glass
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 66 (PA66)
;
Nylon 66, 50% Glass Fiber Filled
Material Notes:
50% Long fiber glass reinforced black Nylon 6.6, heat stabilized for injection molding applications.
Information provided by Polyram.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.58
g/cc
0.0571
lb/in³
ISO 1183
Moisture Absorption at Equilibrium
1.0 %
1.0 %
50% RH; ISO 62
Water Absorption at Saturation
3.4 %
3.4 %
ISO 62
Linear Mold Shrinkage
0.0010
-
0.0030
cm/cm
0.0010
-
0.0030
in/in
ISO 2577
Mechanical Properties
Metric
English
Comments
Tensile Strength, Yield
230
MPa
33400
psi
ISO 527
Elongation at Break
1.5 %
1.5 %
ISO 527
Tensile Modulus
18.0
GPa
2610
ksi
ISO 527
Flexural Strength
380
MPa
55100
psi
ISO 178
Flexural Modulus
16.5
GPa
2390
ksi
ISO 178
Izod Impact, Notched (ISO)
25.0
kJ/m²
11.9
ft-lb/in²
ISO 180
Charpy Impact Unnotched
10.0
J/cm²
47.6
ft-lb/in²
ISO 179
Charpy Impact, Notched
2.80
J/cm²
13.3
ft-lb/in²
ISO 179
Thermal Properties
Metric
English
Comments
Deflection Temperature at 1.8 MPa (264 psi)
253
°C
487
°F
ISO 75
Flammability, UL94
HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
RTP Company RTP 399 X 102186 Polycarbonate (PC), Carbon Fiber - Glass Fiber
RTP Company RTP 1026 Polybutylene Terephthalate (PBT) Glass Fiber/Glass Bead Blend
Polyram Polytron P20B11 Polypropylene, 20% Long Fiber Glass
NRI Syntho-Glass® 24 Fiberglass Mat
NRI Solar-Wrap Fiberglass wrap
PPOLYR936 / 126733
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.