MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

Cookson Group Plaskon® SMT-B-1F Epoxy Molding Compound for PBGAs  (discontinued **)
Categories: Polymer; Thermoset; Epoxy; Epoxy Molding Compound

Material Notes: Test specimens were transfer molded and post cured 4 hours at 175°C.

An epoxy molding compound optimized specifically for PBGA applications. It has the same unique resin system as SMT-B-1, which minimizes warpage and enables trouble-free molding onto rigid and flexible laminate substrates. Faster cure speed for shorter cure times in multi-plunger and automolding equipment; Improved wire sweep performance (lower viscosity); Reduced post mold cure times; Improved warp performance; Lower moisture absorption

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.91 g/cc0.0690 lb/in³
Viscosity 7000 cP
@Temperature 175 °C
7000 cP
@Temperature 347 °F
Shimadzu Viscosity, 1000 psi
Spiral Flow 79.0 cm31.1 in175°C/1000 psi
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 8282
Flexural Strength 68.0 MPa9860 psi
Flexural Modulus 15.0 GPa2180 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 3.20e+16 ohm-cm3.20e+16 ohm-cm
Dielectric Constant 3.9
@Frequency 1000 Hz
3.9
@Frequency 1000 Hz
Dielectric Strength 28.0 kV/mm711 kV/in
 
Thermal PropertiesMetricEnglishComments
CTE, linear 12.0 µm/m-°C
@Temperature 20.0 °C
6.67 µin/in-°F
@Temperature 68.0 °F
CTE, linear, Transverse to Flow 57.0 µm/m-°C
@Temperature 20.0 °C
31.7 µin/in-°F
@Temperature 68.0 °F
Thermal Conductivity 0.700 W/m-K4.86 BTU-in/hr-ft²-°F
Glass Transition Temp, Tg 220 °C428 °F
Flammability, UL94  V-0
@Thickness 3.20 mm
V-0
@Thickness 0.126 in
 V-0
@Thickness 3.20 mm
V-0
@Thickness 0.126 in
 
Processing PropertiesMetricEnglishComments
Processing Temperature 170 - 185 °C338 - 365 °FMolding temperature

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Cookson Group Plaskon® SMT-B-1RC (146.403) Epoxy Molding Compound for PBGAs
Master Bond LED405Med One component, nanosilica filled LED curable system
Cookson Group Plaskon® SMT-B-2FPI Molding Compound for PBGA and CSP
NuSil Lightspan™ LS-8941 Silicone, Optical Adhesive Elastomer
Overview of materials for Epoxy, Thermally Conductive

PCOOK330 / 21426

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.