MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Borealis Daplen™ EF040AE TPO Compound  (discontinued **)
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Olefinic Elastomer (TPO); Polypropylene (PP); TPO

Material Notes: Daplen EF040AE is a elastomer modified polypropylene compound intended for injection molding. Daplen EF040AE is a material with excellent impact/stiffness ratio. Thanks to its low thermal expansion this material is suitable to mold parts requiring low change of dimensions over a broad temperature range. The product is optimized to give good surface aesthetics..

Daplen EF040AE has been developed for automotive exterior applications, bumpers, and exterior trims.

Information provided by the Manufacturer.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.910 g/cc0.0329 lb/in³ISO 1183
Linear Mold Shrinkage 0.0095 cm/cm0.0095 in/inBorealis Method
Melt Flow 22 g/10 min
@Load 2.16 kg,
Temperature 230 °C
22 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 18.0 MPa2610 psiAt 50 mm/min; ISO 527-2
Elongation at Break 330 %330 %At 50 mm/min; ISO 527-2
Elongation at Yield 8.5 %8.5 %At 50 mm/min; ISO 527-2
Tensile Modulus 1.04 GPa151 ksiAt 1 mm/min; ISO 527-2
Flexural Strength 21.0 MPa3050 psiISO 178
Flexural Modulus 1.05 GPa152 ksiAt 2 mm/min; ISO 178
Charpy Impact Unnotched NBNBISO 179/1eU
 NB
@Temperature -20.0 °C
NB
@Temperature -4.00 °F
ISO 179/1eU
Charpy Impact, Notched 4.00 J/cm²19.0 ft-lb/in²ISO 179/1eA
 0.400 J/cm²
@Temperature -30.0 °C
1.90 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 0.550 J/cm²
@Temperature -20.0 °C
2.62 ft-lb/in²
@Temperature -4.00 °F
ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 88.0 °C190 °FISO 75-2
Vicat Softening Point 138 °C280 °FA (10N); ISO 306
Shrinkage 0.15 %
@Temperature 90.0 °C,
Time 7200 sec
0.15 %
@Temperature 194 °F,
Time 2.00 hour
Post Shrinkage; Borealis Method
 
Processing PropertiesMetricEnglishComments
Melt Temperature 220 - 260 °C428 - 500 °FPolymer Mass Temp
Mold Temperature 30.0 - 50.0 °C86.0 - 122 °F

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Chengdu Polyster H4040 Thermoplastic Polyether-ester Elastomer (TPEE)
Envalior Arnitel® PM381 TPC-ET, Extrusion Grade
Chengdu Polyster H4543 Thermoplastic Polyether-ester Elastomer (TPEE)
Borealis Daplen™ EE109AE TPO Compound
Barlog Plastics KEBAFLEX P D40.3 Polyester-Elastomer, Shore D40

PBOREA156 / 27463

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.