MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AISI Type S21800 Stainless Steel
Categories: Metal; Ferrous Metal; Heat Resisting; Stainless Steel; T S20000 Series Stainless Steel

Material Notes: Galling and wear resistant, austenitic. Corrosion resistance better than type 304 in most media and pitting resistance superior than type 316. Room temperature yield strength about 2 times type 304. Excellent high-temperature oxidation resistance and low-temperature impact resistance. Applications include valve stems, seats and trim, nuts and bolts, screening, chain drive systems, and pins, bushings, and roller bearings. 2317 MPa fracture strength.

Key Words: UNS S21800, ASME Code Case 1817, ASTM A193 (grade B8S), ASTM A194 (grade 8S), ASTM A276, ASTM A479, ASTM A580
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.61 g/cc0.275 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 200200Annealed bar.
 110
@Temperature 870 °C
110
@Temperature 1600 °F
Annealed bar.
 143
@Temperature 760 °C
143
@Temperature 1400 °F
Annealed bar.
 144
@Temperature 650 °C
144
@Temperature 1200 °F
Annealed bar.
 145
@Temperature 540 °C
145
@Temperature 1000 °F
Annealed bar.
 148
@Temperature 425 °C
148
@Temperature 797 °F
Annealed bar.
 155
@Temperature 315 °C
155
@Temperature 599 °F
Annealed bar.
 168
@Temperature 205 °C
168
@Temperature 401 °F
Annealed bar.
 187
@Temperature 95.0 °C
187
@Temperature 203 °F
Annealed bar.
Hardness, Knoop 222222Converted from Brinell
 128
@Temperature 870 °C
128
@Temperature 1600 °F
Converted from Brinell
 163
@Temperature 760 °C
163
@Temperature 1400 °F
Converted from Brinell
 164
@Temperature 650 °C
164
@Temperature 1200 °F
Converted from Brinell
 165
@Temperature 540 °C
165
@Temperature 1000 °F
Converted from Brinell
 168
@Temperature 425 °C
168
@Temperature 797 °F
Converted from Brinell
 175
@Temperature 315 °C
175
@Temperature 599 °F
Converted from Brinell
 189
@Temperature 205 °C
189
@Temperature 401 °F
Converted from Brinell
 209
@Temperature 95.0 °C
209
@Temperature 203 °F
Converted from Brinell
Hardness, Rockwell B 9292Converted from Brinell
 63
@Temperature 870 °C
63
@Temperature 1600 °F
Converted from Brinell
 78
@Temperature 540 °C
78
@Temperature 1000 °F
Converted from Brinell
 78
@Temperature 650 °C
78
@Temperature 1200 °F
Converted from Brinell
 78
@Temperature 760 °C
78
@Temperature 1400 °F
Converted from Brinell
 79
@Temperature 425 °C
79
@Temperature 797 °F
Converted from Brinell
 82
@Temperature 315 °C
82
@Temperature 599 °F
Converted from Brinell
 85
@Temperature 205 °C
85
@Temperature 401 °F
Converted from Brinell
 90
@Temperature 95.0 °C
90
@Temperature 203 °F
Converted from Brinell
Hardness, Vickers 210210Converted from Brinell
 114
@Temperature 870 °C
114
@Temperature 1600 °F
Converted from Brinell
 149
@Temperature 760 °C
149
@Temperature 1400 °F
Converted from Brinell
 150
@Temperature 650 °C
150
@Temperature 1200 °F
Converted from Brinell
 151
@Temperature 540 °C
151
@Temperature 1000 °F
Converted from Brinell
 154
@Temperature 425 °C
154
@Temperature 797 °F
Converted from Brinell
 162
@Temperature 315 °C
162
@Temperature 599 °F
Converted from Brinell
 176
@Temperature 205 °C
176
@Temperature 401 °F
Converted from Brinell
 196
@Temperature 95.0 °C
196
@Temperature 203 °F
Converted from Brinell
Tensile Strength, Ultimate 734 MPa106000 psiAnnealed bar.
 754 MPa109000 psi
 208 MPa
@Temperature 870 °C
30200 psi
@Temperature 1600 °F
Annealed bar.
 255 MPa
@Temperature 815 °C
37000 psi
@Temperature 1500 °F
Annealed bar.
 343 MPa
@Temperature 760 °C
49700 psi
@Temperature 1400 °F
Annealed bar.
 407 MPa
@Temperature 705 °C
59000 psi
@Temperature 1300 °F
Annealed bar.
 459 MPa
@Temperature 650 °C
66600 psi
@Temperature 1200 °F
Annealed bar.
 494 MPa
@Temperature 595 °C
71600 psi
@Temperature 1100 °F
Annealed bar.
 520 MPa
@Temperature 540 °C
75400 psi
@Temperature 1000 °F
Annealed bar.
 532 MPa
@Temperature 480 °C
77200 psi
@Temperature 896 °F
Annealed bar.
 540 MPa
@Temperature 425 °C
78300 psi
@Temperature 797 °F
Annealed bar.
 548 MPa
@Temperature 370 °C
79500 psi
@Temperature 698 °F
Annealed bar.
 555 MPa
@Temperature 315 °C
80500 psi
@Temperature 599 °F
Annealed bar.
 566 MPa
@Temperature 260 °C
82100 psi
@Temperature 500 °F
Annealed bar.
 582 MPa
@Temperature 205 °C
84400 psi
@Temperature 401 °F
Annealed bar.
 620 MPa
@Temperature 150 °C
89900 psi
@Temperature 302 °F
Annealed bar.
 640 MPa
@Temperature 95.0 °C
92800 psi
@Temperature 203 °F
Annealed bar.
 883 MPa
@Temperature -18.0 °C
128000 psi
@Temperature -0.400 °F
 1023 MPa
@Temperature -73.0 °C
148400 psi
@Temperature -99.4 °F
 1156 MPa
@Temperature -130 °C
167700 psi
@Temperature -202 °F
 1405 MPa
@Temperature -255 °C
203800 psi
@Temperature -427 °F
 1502 MPa
@Temperature -195 °C
217800 psi
@Temperature -319 °F
Tensile Strength, Yield  390 MPa
@Strain 0.2 %
56600 psi
@Strain 0.2 %
Annealed bar
 401 MPa
@Strain 0.2 %
58200 psi
@Strain 0.2 %
 113 MPa
@Strain 0.2 %,
Temperature 870 °C
16400 psi
@Strain 0.2 %,
Temperature 1600 °F
Annealed bar
 164 MPa
@Strain 0.2 %,
Temperature 815 °C
23800 psi
@Strain 0.2 %,
Temperature 1500 °F
Annealed bar
 174 MPa
@Strain 0.2 %,
Temperature 760 °C
25200 psi
@Strain 0.2 %,
Temperature 1400 °F
Annealed bar
 189 MPa
@Strain 0.2 %,
Temperature 705 °C
27400 psi
@Strain 0.2 %,
Temperature 1300 °F
Annealed bar
 193 MPa
@Strain 0.2 %,
Temperature 540 °C
28000 psi
@Strain 0.2 %,
Temperature 1000 °F
Annealed bar
 194 MPa
@Strain 0.2 %,
Temperature 650 °C
28100 psi
@Strain 0.2 %,
Temperature 1200 °F
Annealed bar
 195 MPa
@Strain 0.2 %,
Temperature 480 °C
28300 psi
@Strain 0.2 %,
Temperature 896 °F
Annealed bar
 198 MPa
@Strain 0.2 %,
Temperature 595 °C
28700 psi
@Strain 0.2 %,
Temperature 1100 °F
Annealed bar
 200 MPa
@Strain 0.2 %,
Temperature 425 °C
29000 psi
@Strain 0.2 %,
Temperature 797 °F
Annealed bar
 201 MPa
@Strain 0.2 %,
Temperature 370 °C
29200 psi
@Strain 0.2 %,
Temperature 698 °F
Annealed bar
 205 MPa
@Strain 0.2 %,
Temperature 315 °C
29700 psi
@Strain 0.2 %,
Temperature 599 °F
Annealed bar
 221 MPa
@Strain 0.2 %,
Temperature 260 °C
32100 psi
@Strain 0.2 %,
Temperature 500 °F
Annealed bar
 226 MPa
@Strain 0.2 %,
Temperature 205 °C
32800 psi
@Strain 0.2 %,
Temperature 401 °F
Annealed bar
 261 MPa
@Strain 0.2 %,
Temperature 150 °C
37900 psi
@Strain 0.2 %,
Temperature 302 °F
Annealed bar
 306 MPa
@Strain 0.2 %,
Temperature 95.0 °C
44400 psi
@Strain 0.2 %,
Temperature 203 °F
Annealed bar
 464 MPa
@Strain 0.2 %,
Temperature -18.0 °C
67300 psi
@Strain 0.2 %,
Temperature -0.400 °F
 537 MPa
@Strain 0.2 %,
Temperature -73.0 °C
77900 psi
@Strain 0.2 %,
Temperature -99.4 °F
 603 MPa
@Strain 0.2 %,
Temperature -130 °C
87500 psi
@Strain 0.2 %,
Temperature -202 °F
 699 MPa
@Strain 0.2 %,
Temperature -195 °C
101000 psi
@Strain 0.2 %,
Temperature -319 °F
 864 MPa
@Strain 0.2 %,
Temperature -255 °C
125000 psi
@Strain 0.2 %,
Temperature -427 °F
Elongation at Break 61.7 %61.7 %Annealed bar. Gage length is 4 times diameter.
 66.4 %66.4 %in 25 mm
 23.5 %
@Temperature -255 °C
23.5 %
@Temperature -427 °F
in 25 mm
 41.4 %
@Temperature 705 °C
41.4 %
@Temperature 1300 °F
Annealed bar. Gage length is 4 times diameter.
 47.1 %
@Temperature 760 °C
47.1 %
@Temperature 1400 °F
Annealed bar. Gage length is 4 times diameter.
 48.2 %
@Temperature 650 °C
48.2 %
@Temperature 1200 °F
Annealed bar. Gage length is 4 times diameter.
 48.7 %
@Temperature 595 °C
48.7 %
@Temperature 1100 °F
Annealed bar. Gage length is 4 times diameter.
 52.2 %
@Temperature 540 °C
52.2 %
@Temperature 1000 °F
Annealed bar. Gage length is 4 times diameter.
 53.9 %
@Temperature 480 °C
53.9 %
@Temperature 896 °F
Annealed bar. Gage length is 4 times diameter.
 56.5 %
@Temperature 425 °C
56.5 %
@Temperature 797 °F
Annealed bar. Gage length is 4 times diameter.
 59.1 %
@Temperature 370 °C
59.1 %
@Temperature 698 °F
Annealed bar. Gage length is 4 times diameter.
 59.5 %
@Temperature -195 °C
59.5 %
@Temperature -319 °F
in 25 mm
 59.6 %
@Temperature 315 °C
59.6 %
@Temperature 599 °F
Annealed bar. Gage length is 4 times diameter.
 61.5 %
@Temperature 260 °C
61.5 %
@Temperature 500 °F
Annealed bar. Gage length is 4 times diameter.
 62.4 %
@Temperature -130 °C
62.4 %
@Temperature -202 °F
in 25 mm
 63.3 %
@Temperature 95.0 °C
63.3 %
@Temperature 203 °F
Annealed bar. Gage length is 4 times diameter.
 64 %
@Temperature 205 °C
64 %
@Temperature 401 °F
Annealed bar. Gage length is 4 times diameter.
 64.4 %
@Temperature 150 °C
64.4 %
@Temperature 302 °F
Annealed bar. Gage length is 4 times diameter.
 70.5 %
@Temperature -73.0 °C
70.5 %
@Temperature -99.4 °F
in 25 mm
 71.3 %
@Temperature -18.0 °C
71.3 %
@Temperature -0.400 °F
in 25 mm
 72.8 %
@Temperature 815 °C
72.8 %
@Temperature 1500 °F
Annealed bar. Gage length is 4 times diameter.
 72.8 %
@Temperature 870 °C
72.8 %
@Temperature 1600 °F
Annealed bar. Gage length is 4 times diameter.
Modulus of Elasticity 180 GPa26100 ksi
Machinability 23 %23 %Based on 100% machinability for AISI 1212 steel.
Charpy Impact 313 J231 ft-lb
 187 J
@Temperature -195 °C
138 ft-lb
@Temperature -319 °F
 230 J
@Temperature -130 °C
170 ft-lb
@Temperature -202 °F
 267 J
@Temperature -73.0 °C
197 ft-lb
@Temperature -99.4 °F
 293 J
@Temperature -18.0 °C
216 ft-lb
@Temperature -0.400 °F
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000982 ohm-cm
@Temperature 23.0 °C
0.0000982 ohm-cm
@Temperature 73.4 °F
Magnetic Permeability <= 1.02<= 1.02annealed
 <= 1.02<= 1.02cold reduction of 10-40%
 <= 1.05<= 1.05cold reduction of 50-70%
 
Thermal PropertiesMetricEnglishComments
CTE, linear  15.8 µm/m-°C
@Temperature 25.0 - 95.0 °C
8.78 µin/in-°F
@Temperature 77.0 - 203 °F
 16.6 µm/m-°C
@Temperature 205 °C
9.22 µin/in-°F
@Temperature 401 °F
 17.3 µm/m-°C
@Temperature 25.0 - 315 °C
9.61 µin/in-°F
@Temperature 77.0 - 599 °F
 17.6 µm/m-°C
@Temperature 425 °C
9.78 µin/in-°F
@Temperature 797 °F
 18.0 µm/m-°C
@Temperature 25.0 - 540 °C
10.0 µin/in-°F
@Temperature 77.0 - 1000 °F
 18.5 µm/m-°C
@Temperature 25.0 - 650 °C
10.3 µin/in-°F
@Temperature 77.0 - 1200 °F
 18.9 µm/m-°C
@Temperature 25.0 - 760 °C
10.5 µin/in-°F
@Temperature 77.0 - 1400 °F
 19.3 µm/m-°C
@Temperature 25.0 - 870 °C
10.7 µin/in-°F
@Temperature 77.0 - 1600 °F
 19.8 µm/m-°C
@Temperature 25.0 - 980 °C
11.0 µin/in-°F
@Temperature 77.0 - 1800 °F
Specific Heat Capacity 0.480 J/g-°C0.115 BTU/lb-°FTypical value for stainless steel.
Thermal Conductivity 20.7 W/m-K144 BTU-in/hr-ft²-°FTypical value for stainless steel.
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.10 %<= 0.10 %
Chromium, Cr 16 - 18 %16 - 18 %
Iron, Fe 59.15 - 65.42 %59.15 - 65.42 %As Balance
Manganese, Mn 7.0 - 9.0 %7.0 - 9.0 %
Nickel, Ni 8.0 - 9.0 %8.0 - 9.0 %
Nitrogen, N 0.080 - 0.18 %0.080 - 0.18 %
Phosphorus, P <= 0.040 %<= 0.040 %
Silicon, Si 3.5 - 4.5 %3.5 - 4.5 %
Sulfur, S <= 0.030 %<= 0.030 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Cobalt Alloy
Carpenter Gall-Tough® Stainless
Cast Stainless Steel CF10SMnN, ASTM A743
AISI Type S21800 Stainless Steel 105 mm annealed bar
Carlson Nitronic® 60® Austenitic Stainless Steel

MQM21AA / 13598

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.