MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Goodfellow Nickel 55/Titanium 45 Shape Memory Alloy
Categories: Metal; Nonferrous Metal; Nickel Alloy

Material Notes: Shape memory alloy is a description applied to that group of metallic materials which show the ability to return to the previously defined shape or size when subjected to the correct thermal procedure. Uses include blood clot filters, cryogenic coupling rings, proportional control valves and orthodontic correction.

Information provided by Goodfellow.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 6.50 g/cc0.235 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 1140 MPa165000 psi
Elongation at Break 15 - 40 %15 - 40 %
Tensile Modulus 60.0 - 90.0 GPa8700 - 13100 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000100 ohm-cm0.0000100 ohm-cmAustenitic
 0.0000800 ohm-cm0.0000800 ohm-cmMartensitic
 
Thermal PropertiesMetricEnglishComments
CTE, linear  6.60 µm/m-°C
@Temperature 20.0 °C
3.67 µin/in-°F
@Temperature 68.0 °F
Martensitic
 11.0 µm/m-°C
@Temperature 20.0 °C
6.11 µin/in-°F
@Temperature 68.0 °F
Austenitic
Thermal Conductivity 8.60 W/m-K59.7 BTU-in/hr-ft²-°FMartensitic
 18.0 W/m-K125 BTU-in/hr-ft²-°FAustenitic
Melting Point 1310 °C2390 °F
 
Component Elements PropertiesMetricEnglishComments
Nickel, Ni 55 %55 %
Titanium, Ti 45 %45 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Nitinol - NiTi Shape Memory Alloy; High-Temperature Phase
Nitinol - NiTi Shape Memory Alloy; Low-Temperature Phase
Goodfellow Nickel 70/Titanium 30 Alloy
Special Metals Nitinol Body-Temperature Ni-Ti alloy
Special Metals Nitinol High-Temperature Shape Memory Ni-Ti alloy Ribbon

NGOODF189 / 16259

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.