Entec Hylex® P1340L2 HB Polycarbonate
Categories:
Polymer
;
Thermoplastic
;
Polycarbonate (PC)
;
Polycarbonate, Unreinforced, Flame Retardant
Material Notes:
POLYCARBONATE, HIGH MELT FLOW, UV STABILIZED, UL94 HB
Information provided by Entec
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.20
g/cc
1.20
g/cc
ASTM D792
Linear Mold Shrinkage, Flow
0.0050
-
0.0070
cm/cm
0.0050
-
0.0070
in/in
ASTM D955
Melt Flow
40
g/10 min
@Load 1.20 kg,
Temperature 300 °C
40
g/10 min
@Load 2.65 lb,
Temperature 572 °F
ASTM D1238
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
58.0
MPa
8410
psi
ASTM D638
Elongation at Break
110 %
110 %
ASTM D638
Flexural Strength
101
MPa
14600
psi
ASTM D790
Flexural Modulus
2.414
GPa
350.1
ksi
ASTM D790
Izod Impact, Notched
6.93
J/cm
@Thickness 3.17 mm
13.0
ft-lb/in
@Thickness 0.125 in
ASTM D256
Thermal Properties
Metric
English
Comments
Deflection Temperature at 1.8 MPa (264 psi)
124
°C
255
°F
Unannealed; ASTM D648
Flammability, UL94
HB
HB
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Entec Hylex® P1010L2 HB Polycarbonate
Entec Hylex® P1325L1 HB Polycarbonate
Entec Hylex® P1007L1 HB Polycarbonate
Entec Hylex® P1017L2 HB Polycarbonate
Entec Hylex® P1010L1 HB Polycarbonate
PENT399 / 186990
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.