MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Trinseo Magnum™ 9555 ABS, High Impact  (discontinued **)
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Heat Resistant, Molded

Material Notes: MAGNUM® ABS resins are thermoplastic materials which provide an excellent balance of processability, impact resistance and heat resistance as imparted by the various polymer compositions. MAGNUM ABS resin are available in a wide range of melt flow rates, impact strength and heat resistance for both high and low gloss applications manufactured by injection molding, sheet or profile extrusion and thermoforming.

The MAGNUM 9000 series of high gloss ABS resins are designed to offer a wide range of impact strengths and melt flow rates to meet the needs of the durables injection molding markets. The 9000 series products offer typical Izod impact strength values from 210 to 400 J/m and melt flow rates ranging from 2.5 to 7.0 g/10min. The gloss values are typically greater than 95% on the 60. Gardner scale for the highest gloss resins and greater than 90% for those products having a broader range of gloss.

MAGNUM 9555 ABS resin offers a broader range of gloss while maintaining high impact strength with a medium melt flow rate.

Data provided by Dow Chemical.

Key Words: Poly(Acrylonitrile Butadiene Styrene)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.04 g/cc0.0376 lb/in³ASTM Data
Linear Mold Shrinkage 0.0055 cm/cm0.0055 in/in
Melt Flow 5.0 g/10 min
@Load 3.80 kg,
Temperature 230 °C
5.0 g/10 min
@Load 8.38 lb,
Temperature 446 °F
ASTM Data
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 107107
Tensile Strength, Ultimate 31.0 MPa4500 psiASTM Data
Tensile Strength, Yield 44.8 MPa6500 psiASTM Data
Elongation at Break 40 %40 %ASTM Data
Elongation at Yield 2.3 %2.3 %ISO Data
Tensile Modulus 2.24 GPa325 ksiASTM Data
Izod Impact, Notched 3.20 J/cm5.99 ft-lb/inASTM Data
Charpy Impact Unnotched NBNBISO Data
 NBNBISO Data, Low Temp
Charpy Impact, Notched 0.900 J/cm²4.28 ft-lb/in²ISO Data, Low Temp
 2.90 J/cm²13.8 ft-lb/in²ISO Data
Instrumented Impact Total Energy 55.0 J
@Temperature 23.0 °C
40.6 ft-lb
@Temperature 73.4 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 91.0 µm/m-°C
@Temperature 20.0 °C
50.6 µin/in-°F
@Temperature 68.0 °F
ISO data
Deflection Temperature at 0.46 MPa (66 psi) 92.0 °C198 °FUnannealed; ASTM Data
Deflection Temperature at 1.8 MPa (264 psi) 77.0 °C171 °FUnannealed; 103°C (217°F) annealed; ASTM Data
Vicat Softening Point 106 °C223 °F
Flammability, UL94 HB
@Thickness 1.47 mm
HB
@Thickness 0.0579 in
 
Optical PropertiesMetricEnglishComments
Gloss 90 %90 %Gardner Gloss, 60°

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LG Chemical HI100 ABS, High Impact
Covestro Bayblend® T65 XF Polycarbonate + ABS
Covestro Bayblend® T80 XG PC/ABS Blend
LG Chemical HI100H ABS, High Impact, High Toughness
Trinseo Magnum™ 9020 ABS, High Gloss

PZZDW112 / 34343

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.