MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Envalior Stanyl® TS300 PA46
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 46 (PA46); Nylon 46, Unreinforced

Material Notes:

Former DSM Engineering Plastics product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.18 g/cc0.0426 lb/in³dry; ISO 1183
Moisture Absorption 3.70 %3.70 %Sim. To ISO 62
Linear Mold Shrinkage, Flow 0.020 cm/cm0.020 in/inSim. To ISO 294-4
Linear Mold Shrinkage, Transverse 0.020 cm/cm0.020 in/inSim. To ISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 55.0 MPa7980 psicond; ISO 527-1/-2
 100 MPa14500 psidry; ISO 527-1/-2
 30.0 MPa
@Temperature 200 °C
4350 psi
@Temperature 392 °F
ISO 527-1/-2
 35.0 MPa
@Temperature 180 °C
5080 psi
@Temperature 356 °F
ISO 527-1/-2
 40.0 MPa
@Temperature 160 °C
5800 psi
@Temperature 320 °F
ISO 527-1/-2
 50.0 MPa
@Temperature 120 °C
7250 psi
@Temperature 248 °F
ISO 527-1/-2
Elongation at Break 40 %40 %dry; ISO 527-1/-2
 >= 50 %>= 50 %cond; ISO 527-1/-2
 >= 50 %
@Temperature 120 °C
>= 50 %
@Temperature 248 °F
ISO 527-1/-2
 >= 50 %
@Temperature 160 °C
>= 50 %
@Temperature 320 °F
ISO 527-1/-2
 >= 50 %
@Temperature 180 °C
>= 50 %
@Temperature 356 °F
ISO 527-1/-2
 >= 50 %
@Temperature 200 °C
>= 50 %
@Temperature 392 °F
ISO 527-1/-2
Tensile Modulus 1.00 GPa145 ksicond; ISO 527-1/-2
 3.30 GPa479 ksidry; ISO 527-1/-2
 0.500 GPa
@Temperature 200 °C
72.5 ksi
@Temperature 392 °F
ISO 527-1/-2
 0.600 GPa
@Temperature 180 °C
87.0 ksi
@Temperature 356 °F
ISO 527-1/-2
 0.650 GPa
@Temperature 160 °C
94.3 ksi
@Temperature 320 °F
ISO 527-1/-2
 0.800 GPa
@Temperature 120 °C
116 ksi
@Temperature 248 °F
ISO 527-1/-2
Flexural Modulus 0.900 GPa131 ksicond; ISO 178
 3.00 GPa435 ksidry; ISO 178
 0.600 GPa
@Temperature 160 °C
87.0 ksi
@Temperature 320 °F
ISO 178
 0.800 GPa
@Temperature 120 °C
116 ksi
@Temperature 248 °F
ISO 178
Izod Impact Resistance  0.400 J/cm²
@Temperature -40.0 °C
1.90 ft-lb/in²
@Temperature -40.0 °F
cond; ISO 180/1A
 0.400 J/cm²
@Temperature -40.0 °C
1.90 ft-lb/in²
@Temperature -40.0 °F
dry; ISO 180/1A
 1.00 J/cm²
@Temperature 23.0 °C
4.76 ft-lb/in²
@Temperature 73.4 °F
dry; ISO 180/1A
 3.50 J/cm²
@Temperature 23.0 °C
16.7 ft-lb/in²
@Temperature 73.4 °F
cond; ISO 180/1A
Charpy Impact Unnotched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
cond; ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
cond; ISO 179/1eU
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
dry; ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
dry; ISO 179/1eU
Charpy Impact, Notched  0.400 J/cm²
@Temperature -30.0 °C
1.90 ft-lb/in²
@Temperature -22.0 °F
cond; ISO 179/1eA
 0.400 J/cm²
@Temperature -30.0 °C
1.90 ft-lb/in²
@Temperature -22.0 °F
dry; ISO 179/1eA
 1.00 J/cm²
@Temperature 23.0 °C
4.76 ft-lb/in²
@Temperature 73.4 °F
dry; ISO 179/1eA
 3.50 J/cm²
@Temperature 23.0 °C
16.7 ft-lb/in²
@Temperature 73.4 °F
cond; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+12 ohm-cm1.00e+12 ohm-cmcond; IEC 60093
 1.00e+15 ohm-cm1.00e+15 ohm-cmdry; IEC 60093
Dielectric Strength 20.0 kV/mm508 kV/incond; IEC 60243-1
 25.0 kV/mm635 kV/indry; IEC 60243-1
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 85.0 µm/m-°C47.2 µin/in-°Fdry; ISO 11359-1/-2
CTE, linear, Transverse to Flow 110 µm/m-°C61.1 µin/in-°Fdry; ISO 11359-1/-2
Melting Point 295 °C563 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 190 °C374 °Fdry; ISO 75-1/-2
Flammability, UL94  V-2
@Thickness 1.50 mm
V-2
@Thickness 0.0591 in
dry; IEC 60695-11-10
 V-2
@Thickness 0.750 mm
V-2
@Thickness 0.0295 in
dry; IEC 60695-11-10

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
BASF Ultramid® A3K BK 00464 PA66 (Conditioned)
Envalior Stanyl® TE300 PA46
Envalior Stanyl® TW341-N PA46
Overview of materials for Nylon 46, Unreinforced
BASF Ultraform® H2320 004 POM

PDSM9902 / 161523

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.