  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Teknor Apex APEX® 84842 Polyvinyl Chloride, Flexible
Categories: Polymer; Thermoplastic; Vinyl (PVC); PVC, Flexible Grade; PVC, Wire and Cable Grade

Material Notes: Notes: 105°C Insulation; High Heat Resistance; Sunlight Resistant (720 hours); RoHS Compliant

Forms: Pellets

Uses: Cable Jacketing; Outdoor Applications

Wire Types: CXTW; SPT-1W; STW; XTW; SJTW; SPT-2W

Agency Ratings: UL 62; UL QMTT2 .E73402

Information Provided by Teknor Apex

Key Words: PVC
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.33 g/cc1.33 g/ccASTM D792
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 868615 seconds; ASTM D2240
Tensile Strength at Break 17.9 MPa2600 psiASTM D638
Elongation at Break 360 %360 %ASTM D638
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.60e+13 ohm-cm1.60e+13 ohm-cmASTM D257
Dielectric Constant  3.06
@Frequency 1e+6 Hz
3.06
@Frequency 1e+6 Hz
ASTM D150
 4.9
@Frequency 1000 Hz
4.9
@Frequency 1000 Hz
ASTM D150
Dissipation Factor  0.075
@Frequency 1e+6 Hz
0.075
@Frequency 1e+6 Hz
ASTM D150
 0.096
@Frequency 1000 Hz
0.096
@Frequency 1000 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 105 °C221 °FContinuous Use; ASTM D794
Brittleness Temperature -30.0 °C-22.0 °FASTM D746
Oxygen Index 29 %29 %ASTM D2863
 
Descriptive Properties
AppearanceOpaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Teknor Apex APEX® 80851 Polyvinyl Chloride, Flexible
Teknor Apex APEX® 80457 Polyvinyl Chloride, Flexible
Teknor Apex APEX® 4167 Polyvinyl Chloride, Flexible
Teknor Apex APEX® 4130 Polyvinyl Chloride, Flexible
Teknor Apex APEX® 327 Polyvinyl Chloride, Flexible

PTEKNO447 / 128624

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.