MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Axiall Suprel® SVA 9812 Rigid PVC, Extrusion  (discontinued **)
Categories: Polymer; Thermoplastic; Vinyl (PVC)

Material Notes: Georgia Gulf Suprel® SVA 9812 Alloy is an extrusion grade thermoplastic designed for sheet or profile applications requiring high impact resistance. Key features of Suprel 9812 alloy are flame retardance and excellent toughness at both room temperature and low temperatures. Suprel 9812 has good extrusion characteristics including good thermal stability and high gloss. It is particularly well suited for profile extrusion because the combination of low die swell, good melt strength and good melt stiffness allow easy sizing of extruded profiles. Suprel 9812 alloy is available in a full range of colors, or as un-pigmented "natural" for coloring on-line with concentrates. Typical applications include extruded sheet or profiles for use in construction, automotive, recreation, telecommunications or electrical products. Suprel 9812 can be used in exterior, weatherable applications if appropriate pigmentation is included.

Information provided by Georgia Gulf

Georgia Gulf became Axiall Corporation, which was later acquired by Westlake Plastics. This specific grade is discontinued.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.25 g/cc1.25 g/ccASTM D-792
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 747415 Seconds Delay; ASTM D-2246
 7979Instantaneous; ASTM D-2246
Tensile Strength, Yield 44.8 MPa6500 psiASTM D-638
Tensile Modulus 2.32 GPa337 ksiASTM D-638
Flexural Strength 63.4 MPa9200 psiASTM D-790
Flexural Modulus 2.25 GPa327 ksiASTM D-790
Izod Impact, Notched  4.27 - 5.87 J/cm
@Thickness 3.17 mm,
Temperature 0.000 °C
8.00 - 11.0 ft-lb/in
@Thickness 0.125 in,
Temperature 32.0 °F
ASTM D-256
 8.54 J/cm
@Thickness 3.17 mm,
Temperature 22.2 °C
16.0 ft-lb/in
@Thickness 0.125 in,
Temperature 72.0 °F
ASTM D-256
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 82.2 °C180 °Fannealed; ASTM D-648
Deflection Temperature at 1.8 MPa (264 psi) 82.2 °C180 °Fannealed; ASTM D-648
Vicat Softening Point 97.8 °C208 °Fannealed; ASTM D-1525A
UL RTI, Electrical 50.0 °C122 °FUL-746B
Flammability, UL94 V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
Flame Spread Index 3535RP; ASTM E-162

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Fainplast Compounds R 220 Rigid PVC, Extrusion
ExxonMobil PP7011L1 Polypropylene Impact Copolymer
Evonik Cyrolon® AR Polycarbonate Sheet
Covestro Makrolon® ET UV530 Polycarbonate
Covestro Makrolon® 3103 Polycarbonate

PGGUL401 / 41677

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.