MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Crucible Steel CSM® S60V (440V) Tool Steel, AISI 440C Modified
Categories: Metal; Ferrous Metal; Tool Steel

Material Notes: CPM S60V is a unique tool steel made by the Crucible Particle Metallurgy process. It is designed from a 440C stainless base analysis with added high carbon and vanadium for exceptionally good wear resistance.
The exceptional wear resistance and good corrosion resistance of CPM S60V make it an excellent candidate to replace 440C and other corrosion and wear resistant materials, particularly where increased wear resistance is a primary concern.

Information provided by Crucible Industries

Key Words: AISI 440C Modified
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.47 g/cc0.270 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C 5858Heat Treated at 1950°F then air cooled
 6060Heat Treated at 1950°F then quenched
 54
@Tempering Temp. 260 - 371 °C
54
@Tempering Temp. 500 - 700 °F
Heat Treated at 1950°F then air cooled and tempered
 55
@Tempering Temp. 260 - 371 °C
55
@Tempering Temp. 500 - 700 °F
Heat Treated at 1950°F then quenched and tempered
 56
@Tempering Temp. 204 °C
56
@Tempering Temp. 400 °F
Heat Treated at 1950°F then air cooled and tempered
 56
@Tempering Temp. 316 - 371 °C
56
@Tempering Temp. 600 - 700 °F
Heat Treated at 2050°F then air cooled and tempered
 58
@Tempering Temp. 204 °C
58
@Tempering Temp. 400 °F
Heat Treated at 2050°F then air cooled and tempered
 58
@Tempering Temp. 204 °C
58
@Tempering Temp. 400 °F
Heat Treated at 1950°F then quenched and tempered
 58
@Tempering Temp. 316 - 371 °C
58
@Tempering Temp. 600 - 700 °F
Heat Treated at 2050°F then quenched and tempered
 60
@Tempering Temp. 204 °C
60
@Tempering Temp. 400 °F
Heat Treated at 2050°F then quenched and tempered
Modulus of Elasticity 207 GPa30000 ksi
Charpy Impact  16.3 J
@Treatment Temp. 1070 °C
12.0 ft-lb
@Treatment Temp. 1950 °F
hardened; C-notch
 21.7 J
@Treatment Temp. 1010 °C
16.0 ft-lb
@Treatment Temp. 1850 °F
hardened; C-notch
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.1 µm/m-°C
@Temperature 21.1 - 204 °C
6.14 µin/in-°F
@Temperature 70.0 - 400 °F
 11.5 µm/m-°C
@Temperature 21.1 - 316 °C
6.37 µin/in-°F
@Temperature 70.0 - 600 °F
 12.2 µm/m-°C
@Temperature 21.1 - 593 °C
6.79 µin/in-°F
@Temperature 70.0 - 1100 °F
Thermal Conductivity 16.7 W/m-K116 BTU-in/hr-ft²-°F
 
Processing PropertiesMetricEnglishComments
Processing Temperature 860 °C1580 °FCritical Thermal Treatment Temperature
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 2.15 %2.15 %
Chromium, Cr 17 %17 %
Iron, Fe 73.5 %73.5 %as balance
Manganese, Mn 0.40 %0.40 %
Molybdenum, Mo 1.0 %1.0 %
Silicon, Si 0.40 %0.40 %
Vanadium, V 5.5 %5.5 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
440C Martensitic Stainless Steel (UNS S44004)
AISI 440 Stainless Steel
Crucible Steel 440C Chromium Steel
ATI Allegheny Ludlum AL 440C™ Martensitic Stainless Steel, UNS S44004
Cast Stainless Steel 440C, ASTM A276

NCRUC945 / 160396

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.