MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Magnesium AZ91C-T4, Cast
Categories: Metal; Nonferrous Metal; Magnesium Alloy

Material Notes: AZ91A, B, C, D, and E have the same nominal composition but differ in ranges and/or specified impurity limits. This alloy is used in sand cast and permanent-mold castings when maximum corrosion resistance is not required.

Key Words: UNS M11914; Mg; European EN 1753 MC 21120; ASTM B 80; ASTM B 403; SAE J465; Old SAE 504 (Ingot UNS M11915)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.81 g/cc0.0654 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 5555500 kg load, 10 mm ball
Hardness, Knoop 7070Estimated from Brinell
Hardness, Rockwell E 6262
Tensile Strength, Ultimate 275 MPa39900 psi
Tensile Strength, Yield 90.0 MPa
@Strain 0.2 %
13100 psi
@Strain 0.2 %
Elongation at Break 15 %15 %in 50 mm
Tensile Modulus 44.8 GPa6500 ksi
Compressive Yield Strength 90.0 MPa13100 psiat 0.2% offset
Ultimate Bearing Strength 415 MPa60200 psi
Bearing Yield Strength 305 MPa44200 psi
Poissons Ratio 0.350.35
Fatigue Strength  60.0 MPa
@# of Cycles 1.00e+8
8700 psi
@# of Cycles 1.00e+8
Notched Fatigue, Rotating Beam, R=-1, Notched, Sand cast
 75.0 MPa
@# of Cycles 1.00e+6
10900 psi
@# of Cycles 1.00e+6
Notched Fatigue, Rotating Beam, R=-1, Notched, Sand cast
 75.0 MPa
@# of Cycles 1.00e+7
10900 psi
@# of Cycles 1.00e+7
Unnotched Fatigue, Krouse plate bending, R=-1, Sand cast
 85.0 MPa
@# of Cycles 1.00e+6
12300 psi
@# of Cycles 1.00e+6
Unnotched Fatigue, Krouse plate bending, R=-1, Sand cast
 85.0 MPa
@# of Cycles 5.00e+8
12300 psi
@# of Cycles 5.00e+8
R.R. Moore Test
 95.0 MPa
@# of Cycles 1.00e+8
13800 psi
@# of Cycles 1.00e+8
Notched Fatigue, Rotating Beam, R=-1, Smooth, Sand cast
 105 MPa
@# of Cycles 100000
15200 psi
@# of Cycles 100000
Unnotched Fatigue, Krouse plate bending, R=-1, Sand cast
 105 MPa
@# of Cycles 1.00e+7
15200 psi
@# of Cycles 1.00e+7
Notched Fatigue, Rotating Beam (R=-1), Smooth, Sand cast
 115 MPa
@# of Cycles 1.00e+6
16700 psi
@# of Cycles 1.00e+6
Notched Fatigue, Rotating Beam, R=-1, Smooth, Sand cast
 135 MPa
@# of Cycles 100000
19600 psi
@# of Cycles 100000
Shear Modulus 17.0 GPa2470 ksi
Charpy Impact 4.10 J3.02 ft-lbV-notch
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000129 ohm-cm0.0000129 ohm-cm(-T6 Temper)
 
Thermal PropertiesMetricEnglishComments
Heat of Fusion 373 J/g160 BTU/lb
CTE, linear  26.0 µm/m-°C
@Temperature 25.0 °C
14.4 µin/in-°F
@Temperature 77.0 °F
 27.2 µm/m-°C
@Temperature 20.0 - 200 °C
15.1 µin/in-°F
@Temperature 68.0 - 392 °F
Specific Heat Capacity 1.047 J/g-°C0.2502 BTU/lb-°F
Thermal Conductivity 72.7 W/m-K505 BTU-in/hr-ft²-°F
Melting Point >= 421 °C>= 790 °FIncipient Melting
Solidus 470 °C878 °F
Liquidus 595 °C1100 °F
 
Processing PropertiesMetricEnglishComments
Casting Temperature 650 - 815 °C1200 - 1500 °FPermanent Mold Casting
 705 - 845 °C1300 - 1550 °FSand Casting
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 8.1 - 9.3 %8.1 - 9.3 %
Copper, Cu <= 0.10 %<= 0.10 %
Magnesium, Mg 90 %90 %As Remainder
Manganese, Mn >= 0.13 %>= 0.13 %
Nickel, Ni <= 0.010 %<= 0.010 %
Silicon, Si <= 0.30 %<= 0.30 %
Zinc, Zn 0.40 - 1.0 %0.40 - 1.0 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Magnesium AZ91C-T6, Cast
Magnesium AZ91C-F, Cast
Magnesium AZ91D-F, Cast
Magnesium AZ91A-F, Die Cast
Magnesium AZ91E-T4, Cast

MMAZ91 / 12335

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.