MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Solvay EF2000 Organosilicate Polymer
Categories: Polymer; Thermoset

Material Notes: EF2000 prepreg matrix is a complex organosilicate polymer suitable for very high temperature applications. The prepreg is typically cured at 180°C (356°F), although lower temperature cures are possible. EF2000 is intended for use as lightweight, disposable heat shields to protect composite structures for periods up to 10 hrs at 400°C (752°C) with short thermal spikes up to 700°C (1292°F). EF2000 is suitable for non-load bearing applications or lightly loaded components with well designed attachment areas.

Features & Benefits:

  • 5 day tack life at 21°C (70°F) with both release films in position
  • 15 days storage at -18°C (0°F)
  • Typical cure 180°C (356°F)
  • Maximum service temperature to 400°C (752°F) for up to 10 hours and short thermal spikes up to 700°C (1292°F)
Property data for EF2000- T300 199g/cm2 3k 2x2 twill carbon fabric

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.85 g/cc0.0668 lb/in³Cured Resin
pH 12.512.5uncured matrix
Storage Temperature -18.0 °C-0.400 °F
 
Mechanical PropertiesMetricEnglishComments
Flexural Strength 30.0 MPa4350 psi0/90° Orientation, Cure: 2 hrs at 180°C + 1 hr at 600°C; CRAG 200
 88.3 MPa12800 psi0/90° Orientation, Cure: 2 hrs at 180°C + 1 hr at 400°C; CRAG 200
 144 MPa20900 psi0/90° Orientation, Cure: 2 hrs at 180°C; CRAG 200
Flexural Modulus 14.0 GPa2030 ksi0/90° Orientation, Cure: 2 hrs at 180°C + 1 hr at 400°C; CRAG 200
 45.0 GPa6530 ksi0/90° Orientation, Cure: 2 hrs at 180°C; CRAG 200
 
Thermal PropertiesMetricEnglishComments
Melting Point 800 °C1470 °F2 hrs at 180°C + 30 mins at 300°C
Maximum Service Temperature, Air 400 °C752 °F< 10 hours
 700 °C1290 °Fshort thermal spikes
 
Processing PropertiesMetricEnglishComments
Shelf Life 0.500 Month0.500 Month

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Pyrotek F-51 Dense Machinable Board
Brandenburger GL-P Thermal Insulation Board
Overview of materials for Thermoplastic Polyimide, Unfilled
DuPont™ Kapton® 500A Polyimide Film, 125 Micron Thickness
DuPont™ Kapton® 500FPC Polyimide Film, 125 Micron Thickness

PCYTED171 / 180473

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.