MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Ascend Performance Materials Vydyne® R220 Nylon 66, 40% Mineral Filled
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 40% Mineral Filled

Material Notes: Vydyne R220 is a 40% mineral-reinforced PA66 resin formulated for improved impact strength. Available in natural, it is an injection-molding grade formulated to retain the inherent processing advantages of unreinforced PA66 while enhancing rigidity, strength and heat resistance. R220 maintains the chemical resistance typical of PA66 to a wide variety of chemicals, gasoline, oils, greases and solvents.

Information provided by Ascend Performance Materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.48 g/cc0.0535 lb/in³DAM; ISO 1183
Water Absorption 1.1 %
@Time 86400 sec
1.1 %
@Time 24.0 hour
DAM; ISO 62
Moisture Absorption at Equilibrium 1.6 %1.6 %DAM to 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.011 cm/cm
@Thickness 2.00 mm
0.011 in/in
@Thickness 0.0787 in
DAM; ISO 294-4
Linear Mold Shrinkage, Transverse 0.010 cm/cm
@Thickness 2.00 mm
0.010 in/in
@Thickness 0.0787 in
DAM; ISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 73.0 MPa10600 psi50% RH; ISO 527-2
 103 MPa14900 psiDAM; ISO 527-2
Elongation at Break 6.0 %6.0 %DAM; ISO 527-2
 30 %30 %50% RH; ISO 527-2
Elongation at Yield 1.5 %1.5 %DAM; ISO 527-2
 16 %16 %50% RH; ISO 527-2
Tensile Modulus 2.60 GPa377 ksi50% RH; ISO 527-2
 6.90 GPa1000 ksiDAM; ISO 527-2
Flexural Strength 50.0 MPa7250 psi50% RH; ISO 178
 124 MPa18000 psiDAM; ISO 178
Flexural Modulus 2.30 GPa334 ksi50% RH; ISO 178
 6.10 GPa885 ksiDAM; ISO 178
Poissons Ratio 0.400.40ISO 527-2
Izod Impact, Notched (ISO)  7.00 kJ/m²
@Temperature -30.0 °C
3.33 ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 180/1A
 7.00 kJ/m²
@Temperature -30.0 °C
3.33 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 180/1A
 9.00 kJ/m²
@Temperature 23.0 °C
4.28 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 180/1A
 16.0 kJ/m²
@Temperature 23.0 °C
7.61 ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 180/1A
Charpy Impact Unnotched  11.0 J/cm²
@Temperature -30.0 °C
52.3 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 179/1eU
 13.0 J/cm²
@Temperature -30.0 °C
61.9 ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 179/1eU
 14.0 J/cm²
@Temperature 23.0 °C
66.6 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eU
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
50% RH; ISO 179/1eU
Charpy Impact, Notched  0.600 J/cm²
@Temperature -30.0 °C
2.86 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 179/1eA
 0.700 J/cm²
@Temperature 23.0 °C
3.33 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eA
 0.800 J/cm²
@Temperature -30.0 °C
3.81 ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 179/1eA
 1.70 J/cm²
@Temperature 23.0 °C
8.09 ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 63.0 µm/m-°C
@Thickness 2.00 mm,
Temperature 35.0 - 55.0 °C
35.0 µin/in-°F
@Thickness 0.0787 in,
Temperature 95.0 - 131 °F
DAM; ISO 11359-2
CTE, linear, Transverse to Flow 60.0 µm/m-°C
@Thickness 2.00 mm,
Temperature 23.0 - 55.0 °C
33.3 µin/in-°F
@Thickness 0.0787 in,
Temperature 73.4 - 131 °F
DAM; ISO 11359-2
Melting Point 258 °C496 °FDAM; ISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 222 °C432 °FUnannealed; DAM; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 118 °C244 °FUnannealed; DAM; ISO 75-2/A
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 280 - 310 °C536 - 590 °FInjection
Middle Barrel Temperature 280 - 310 °C536 - 590 °FInjection
Front Barrel Temperature 280 - 310 °C536 - 590 °FInjection
Nozzle Temperature 280 - 310 °C536 - 590 °FInjection
Melt Temperature 285 - 305 °C545 - 581 °FInjection
Mold Temperature 65.0 - 95.0 °C149 - 203 °FInjection
Drying Temperature 80.0 °C176 °FInjection
Dry Time 4.00 hour4.00 hourInjection
 
Descriptive Properties
AdditiveHeat Stabilizer
Agency RatingsASTM, D4066 PA114M40
 ASTM, D6779 PA114M40
AppearanceNatural Color
Automotive Material SpecificationChrysler MS-DB-41_CPN 2310
 Ford ESB-M4D353-A4
FeaturesChemical Resistant
 Ductile
 Gasoline Resistant
 Good Impact Strength
 Good Strength
 Good Toughness
 Grease Resistant
 High Heat Resistance
 High Rigidity
 Impact Modified
 Oil Resistant
 Solvent Resistant
FormsPellets
Processing MethodInjection Molding
RegionNorth America, Europe, Asia Pacific

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Asahi Kasei Leona™ 54G33 Polyamide 66, GF Reinforced
Asahi Kasei Leona™ 90G60 Polyamide 66, GF Reinforced
Asahi Kasei Leona™ 13G15 Polyamide 66, GF Reinforced
A. Schulman ComAlloy Hiloy® 612 Nylon 6, Glass Reinforced, UL
Ascend Performance Materials Vydyne® R530 NAT Nylon 66, 30% Glass Filled

PASCE9734 / 220837

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.