MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Plastics Group Polifil® C-30 30% Calcium Carbonate-Reinforced Polypropylene
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene with 30% Calcium Carbonate (CaCO3) Filler

Material Notes: Polifil® C series compounds are homopolymer polypropylene resins reinforced with fine particle size calcium carbonate. They combine high impact with stiffness, heat aging, good colorability, resistance to environmental stress-cracking, good surface and low mold shrinkage.

Applications:

  • Appliances
  • Electrical components
  • Housewares
  • Toys
  • Automotive
  • Utility products

Standard processing techniques are applicable.

Information provided by The Plastics Group.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.15 g/cc1.15 g/ccASTM D792
Density 1.15 g/cc0.0415 lb/in³ASTM D792
Filler Content 30 %30 %ASTM D2584
 30.0 %30.0 %TPG WI
Water Absorption 0.000 %
@Time 86400 sec
0.000 %
@Time 24.0 hour
ASTM D570
Linear Mold Shrinkage  0.0090 cm/cm
@Thickness 1.59 mm
0.0090 in/in
@Thickness 0.0625 in
ASTM D955
 0.0120 cm/cm
@Thickness 3.17 mm
0.0120 in/in
@Thickness 0.125 in
ASTM D955
Melt Flow 8.0 - 12 g/10 min8.0 - 12 g/10 min230/2.16; May be specified; ASTM D1238
 8.00 - 12.0 g/10 min
@Load 2.16 kg,
Temperature 230 °C
8.00 - 12.0 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 9898ASTM D785
Hardness, Shore D 75.075.0ASTM D1415
Tensile Strength at Break 25.5 MPa3700 psiASTM D638
Tensile Strength 24.8 MPa3600 psiASTM D638
Elongation at Break 50.0 %50.0 %ASTM D638
Elongation at Yield 6.00 %6.00 %ASTM D638
Tensile Modulus 1.86 GPa270 ksiASTM D638
Flexural Strength 40.0 MPa5800 psiASTM D790
Flexural Modulus 2.07 GPa300 ksiTangent; ASTM D790
 2.07 GPa300 ksitangent; ASTM D790
Izod Impact, Notched 0.320 J/cm0.600 ft-lb/inASTM D256
 0.464 J/cm0.870 ft-lb/inAt 73°F; ASTM D256
Izod Impact, Unnotched 8.54 J/cm16.0 ft-lb/inAt 73°F; ASTM D256
Gardner Impact 1.24 J0.917 ft-lbASTM D3029
 6.78 J
@Thickness 12.7 mm
5.00 ft-lb
@Thickness 0.500 in
tup; ASTM D5420
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 104 °C220 °FASTM D648
 104 °C220 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 60.0 °C140 °FASTM D648
Flammability, UL94 HBHB
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 199 - 210 °C390 - 410 °F
Middle Barrel Temperature 210 - 221 °C410 - 430 °F
Front Barrel Temperature 221 - 232 °C430 - 450 °F
Nozzle Temperature 227 - 232 °C440 - 450 °F
Melt Temperature 204 - 260 °C400 - 500 °F
Mold Temperature 10.0 - 26.7 °C50.0 - 80.0 °F
Drying Temperature 180 - 220 °C
@Time 3600 - 7200 sec
356 - 428 °F
@Time 1.00 - 2.00 hour
Back Pressure 0.345 - 0.689 MPa50.0 - 100 psi
Screw Speed 50.0 - 100 rpm50.0 - 100 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polypropylene with 30% Calcium Carbonate (CaCO3) Filler
Entec Hypro™ F PPH-CC30 Natural Homopolymer Polypropylene, 30% Calcium Carbonate Filled
Entec Hypro™ F PPC-CC30 Natural Copolymer Polypropylene, 30% Calcium Carbonate Filled
Albis Plastics Polypropylene PP 14A12 KR 30 , 30% Calcium Carbonate (CaCO3)
Albis Plastics Polypropylene PP 14A12 CaCO3 30 , 30% Calcium Carbonate (CaCO3)

PPOLI012 / 56916

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.