MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

ChevronTexaco FM NLGI 0 Grease EP
Categories: Fluid; Lubricant; Urea Gellant

Material Notes: Features

Chevron FM Greases EP are high performance, multipurpose food machinery greases that are white in color, odorless, tasteless, and water-resistant. Available in three grades, Chevron FM Greases EP were developed for the food processing and canning industries. Chevron FM Greases EP are a blend of a synthetic polyurea complex thickener and food grade white oils (Group II) containing a highly effective rust inhibitor. They are smooth and buttery in texture, and are slightly tacky.

All grades contain a specially blended higher viscosity white mineral oil that imparts improved adhesive and stringiness properties to the grease.

Applications

Chevron FM Greases EP are multipurpose lubricants for all grease lubricated machinery in canneries, beverage bottlers and canners, potato/corn chip processors, candy manufacturers, meat and poultry packers, frozen food processors, and other food producers and processors. They are specifically recommended for critical applications where there is a possibility of the lubricant becoming an incidental or accidental food ingredient.

NLGI 0 is preferred for low temperature operations,particularly in centralized systems.

Key Words: CPS Number: 230198; MSDS Number: 7882
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Viscosity Measurement 109109Viscosity Index; ASTM D2270
 220220ISO viscosity grade
Saybolt Viscosity at 100°F 1060 SUS1060 SUS
Saybolt Viscosity at 210°F 98 SUS98 SUS
Kinematic Viscosity at 40°C (104°F) 202 cSt202 cStASTM D445
Kinematic Viscosity at 100°C (212°F) 19.4 cSt19.4 cStASTM D445
 
Mechanical PropertiesMetricEnglishComments
Four Ball Wear 0.440 mm0.0173 in
Penetration 370370worked
Penetration P(0), 1/10 mm 347347
Timken Test 6800 g15.0 lb
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 149 °C300 °F
Minimum Service Temperature, Air -40.0 °C-40.0 °F
Pour Point -13.0 °C8.60 °FASTM D97
Flash Point 200 °C392 °FASTM D92
Dropping Point 246 °C475 °F
 
Descriptive Properties
Colorwhite
Lincoln Ventmeter, psig at 30 s, at 0°F0
Lincoln Ventmeter, psig at 30 s, at -22°Ftoo stiff at this temperature to pump through device
Lincoln Ventmeter, psig at 30 s, at 30°F0
Lincoln Ventmeter, psig at 30 s, at 75°F0
Texturesmooth, buttery
Thickener, % / type13 / Polyurea Complex

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

WCHEV099 / 74714

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.