MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

Lord Adhesives CoolTherm™ SC6711/6730 Silicone Encapsulant
Categories: Polymer; Thermoset; Silicone; Silicone Elastomer, for Thermal Management

Material Notes: LORD CoolTherm™ SC-6711/6730 silicone encapsulant is a two-component, thermally conductive encapsulant system with outstanding electrical properties. CoolTherm SC-6711/6730 encapsulant system is an ideal potting compound for any application where rapid heat transfer, high temperature service and a flexible system are required. CoolTherm SC-6730 hardener is blue-green in color and assures thorough mixing by visual examination.

Features: maintains low viscosity for complete and void-free encapsulation. provides thermal conductivity for applications where superior heat dissipation are required. minimizes the possibility of cracking during severe temperature cycling.

All information provided by Lord.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.44 g/cc1.44 g/ccSC-6730 Hardener
 2.20 g/cc2.20 g/ccSC-6711 WHT Silicone Resin
Viscosity  5000 cP
@Temperature 25.0 °C
5000 cP
@Temperature 77.0 °F
SC-6730 Hardener
 30000 cP
@Temperature 25.0 °C
30000 cP
@Temperature 77.0 °F
SC-6711 WHT Silicone Resin
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6060cured
Tensile Strength 5.52 MPa
@Temperature 25.0 °C
800 psi
@Temperature 77.0 °F
cured
Elongation at Break 70 %70 %cured
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+14 ohm-cm
@Temperature 25.0 °C
1.00e+14 ohm-cm
@Temperature 77.0 °F
cured
Dielectric Constant 5.25.2cured
Dielectric Strength 19.7 kV/mm500 kV/incured
Dissipation Factor 0.0200.020cured
 
Thermal PropertiesMetricEnglishComments
CTE, linear 150 µm/m-°C83.3 µin/in-°Fcured
Thermal Conductivity 1.00 W/m-K6.94 BTU-in/hr-ft²-°Fcured, hot die transient method
 
Processing PropertiesMetricEnglishComments
Cure Time 720 - 960 min
@Temperature 25.0 °C
12.0 - 16.0 hour
@Temperature 77.0 °F
mixed
Pot Life 120 - 180 min
@Temperature 25.0 °C
120 - 180 min
@Temperature 77.0 °F
mixed, working life
Shelf Life 6.00 Month
@Temperature 25.0 °C
6.00 Month
@Temperature 77.0 °F
each component, from date of manufacture when stored in original, unopened container
 
Descriptive Properties
AppearanceBlue-green LiquidSC-6730 Hardener
 White PasteSC-6711 WHT Silicone Resin
Usage Level % by weight3mixed

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Lord Adhesives CoolTherm™ SC-6709/6730 Silicone encapsulant system
Lord Adhesives CoolTherm™ SC-6710/6731 Silicone Resin System
Lord Adhesives CoolTherm™ SC6711/6731 Silicone Encapsulant
Lord Adhesives CoolTherm™ SC6711/6732 Silicone Encapsulant
Lord Adhesives CoolTherm™ SC-6712/6730 Silicone Resin System

PLORD9243 / 232599

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.