MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

AISI 1080 Steel, cold drawn, spheroidized annealed, 19-32 mm (0.75-1.25 in) round
Categories: Metal; Ferrous Metal; Carbon Steel; AISI 1000 Series Steel; High Carbon Steel

Material Notes: Similar to AISI 1055 and AISI 1074.

Key Words: UNS G10800, carbon steels
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.85 g/cc0.284 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 192192
Hardness, Knoop 214214Converted from Brinell
Hardness, Rockwell B 9191Converted from Brinell
Hardness, Rockwell C 1111Converted from Brinell hardness. Value below normal HRC range, for comparison purposes only.
Hardness, Vickers 201201Converted from Brinell
Tensile Strength, Ultimate 675 MPa97900 psi
Tensile Strength, Yield 515 MPa74700 psi
Elongation at Break 10 %10 %In 50 mm
Reduction of Area 40 %40 %
Modulus of Elasticity 205 GPa29700 ksiTypical for steel
Bulk Modulus 160 GPa23200 ksiTypical for steel
Poissons Ratio 0.290.29Typical For Steel
Machinability 45 %45 %Based on AISI 1212 steel = 100%
Shear Modulus 80.0 GPa11600 ksiTypical for steel
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000180 ohm-cm
@Temperature 20.0 °C
0.0000180 ohm-cm
@Temperature 68.0 °F
condition of specimen unknown
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.0 µm/m-°C
@Temperature 0.000 - 100 °C
6.11 µin/in-°F
@Temperature 32.0 - 212 °F
 12.2 µm/m-°C
@Temperature 0.000 - 300 °C
6.78 µin/in-°F
@Temperature 32.0 - 572 °F
 13.7 µm/m-°C
@Temperature 0.000 - 500 °C
7.61 µin/in-°F
@Temperature 32.0 - 932 °F
Specific Heat Capacity 0.490 J/g-°C0.117 BTU/lb-°F50-100ºC
Thermal Conductivity 47.7 W/m-K331 BTU-in/hr-ft²-°F0ºC
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.75 - 0.88 %0.75 - 0.88 %
Iron, Fe 98.13 - 98.65 %98.13 - 98.65 %As remainder
Manganese, Mn 0.60 - 0.90 %0.60 - 0.90 %
Phosphorus, P <= 0.040 %<= 0.040 %
Sulfur, S <= 0.050 %<= 0.050 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI 1080 Steel, as rolled
AISI 1144 Steel, hot rolled, 19-32 mm (0.75-1.25 in) round
AISI 1080 Steel, hot rolled, 19-32 mm (0.75-1.25 in) round
AISI 1080 Steel, oil quenched from 815°C (1500°F), tempered at 480°C (900°F)
AISI 1045 Steel, cold drawn, 19-32 mm (0.75-1.25 in) round

M1080F / 7082

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.