MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Polymer Resources PPX-FR1-[color]-EN Modified-PPO, V-0 Flame Retardant, Extrusion Grade
Categories: Polymer; Thermoplastic; Polyphenylene Ether/PPO; Polyphenylene Ether, Heat Resistant

Material Notes: Modified-Polyphenylene Oxide, V-0 Flame Retardant, 190F HDT, Extrusion Grade

Features: • Bromine Free • Chlorine Free
Process: Extrusion
Notes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test samples.

Information provided by Polymer Resources Corporation.

Key Words: UL E113219; Polyphenylene Ether + PS
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.08 g/cc1.08 g/ccASTM D792
Linear Mold Shrinkage 0.0050 - 0.0070 cm/cm0.0050 - 0.0070 in/inASTM D955
Melt Flow 15 - 40 g/10 min
@Load 11.6 kg,
Temperature 250 °C
15 - 40 g/10 min
@Load 25.6 lb,
Temperature 482 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 113113ASTM D785
Tensile Strength at Break 46.9 MPa6800 psiASTM D638
Tensile Strength, Yield 56.5 MPa8200 psiASTM D638
Elongation at Break 50 %50 %ASTM D638
Flexural Strength 89.6 MPa13000 psiASTM D790
Flexural Modulus 2.28 GPa330 ksiASTM D790
Izod Impact, Notched  1.60 J/cm
@Temperature -40.0 °C
3.00 ft-lb/in
@Temperature -40.0 °F
ASTM D256
 3.74 J/cm
@Temperature 22.8 °C
7.00 ft-lb/in
@Temperature 73.0 °F
ASTM D256
Gardner Impact 16.9 J12.5 ft-lbASTM D3029
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+17 ohm-cm1.00e+17 ohm-cmASTM D257
Dielectric Strength 22.0 kV/mm560 kV/inASTM D149
Comparative Tracking Index 250 - 400 V250 - 400 VUL 746
Hot Wire Ignition, HWI  >= 120 sec
@Thickness 1.50 mm
>= 120 sec
@Thickness 0.0591 in
UL 746
 >= 120 sec
@Thickness 1.70 mm
>= 120 sec
@Thickness 0.0669 in
UL 746
 >= 120 sec
@Thickness 3.00 mm
>= 120 sec
@Thickness 0.118 in
UL 746
High Amp Arc Ignition, HAI  60 - 120 arcs
@Thickness 1.50 mm
60 - 120 arcs
@Thickness 0.0591 in
UL 746
 60 - 120 arcs
@Thickness 1.70 mm
60 - 120 arcs
@Thickness 0.0669 in
UL 746
 60 - 120 arcs
@Thickness 3.00 mm
60 - 120 arcs
@Thickness 0.118 in
UL 746
High Voltage Arc-Tracking Rate, HVTR 80.0 - 150 mm/min3.15 - 5.91 in/minUL 746
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 87.8 °C190 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 82.2 °C180 °FASTM D648
UL RTI, Electrical  110 °C
@Thickness 1.50 mm
230 °F
@Thickness 0.0591 in
UL 746
 110 °C
@Thickness 1.70 mm
230 °F
@Thickness 0.0669 in
UL 746
 110 °C
@Thickness 3.00 mm
230 °F
@Thickness 0.118 in
UL 746
UL RTI, Mechanical with Impact  110 °C
@Thickness 1.50 mm
230 °F
@Thickness 0.0591 in
UL 746
 110 °C
@Thickness 1.70 mm
230 °F
@Thickness 0.0669 in
UL 746
 110 °C
@Thickness 3.00 mm
230 °F
@Thickness 0.118 in
UL 746
UL RTI, Mechanical without Impact  95.0 °C
@Thickness 1.50 mm
203 °F
@Thickness 0.0591 in
UL 746
 95.0 °C
@Thickness 1.70 mm
203 °F
@Thickness 0.0669 in
UL 746
 95.0 °C
@Thickness 3.00 mm
203 °F
@Thickness 0.118 in
UL 746
Flammability, UL94  V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
 V-0
@Thickness 3.00 mm
V-0
@Thickness 0.118 in
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature >= 171 °C>= 340 °F
Middle Barrel Temperature >= 188 °C>= 370 °F
Front Barrel Temperature >= 188 °C>= 370 °F
Melt Temperature 193 - 216 °C380 - 420 °F
Drying Temperature 71.1 - 82.2 °C160 - 180 °F
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hour
Vent Depth 0.00254 cm0.00100 in

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Asahi Kasei Xyron® X9653 Modified Polyphenylene Ether
Asahi Kasei Xyron® X0715 Modified Polyphenylene Ether
Asahi Kasei Xyron® A1400 PPE/PA

PPOLYQ208 / 160729

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.