MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Ascend Performance Materials Vydyne® B 45 GF BK EST KW2 PA6-GF45
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 50% Glass Fiber Filled

Material Notes: Vydyne B 45 GF BK EST KW2 is standard flow, organic heat stabilized, 45% glass-fiber reinforced PA6 resin. Available in black, this product is also lubricated for improved machine feed and flow.

Information provided by Ascend Performance Materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.51 g/cc0.0546 lb/in³DAM; ISO 1183
Moisture Absorption at Equilibrium 1.7 %1.7 %DAM to 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0020 cm/cm
@Thickness 2.00 mm
0.0020 in/in
@Thickness 0.0787 in
DAM; ISO 294-4
Linear Mold Shrinkage, Transverse 0.0070 cm/cm
@Thickness 2.00 mm
0.0070 in/in
@Thickness 0.0787 in
DAM; ISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 145 MPa21000 psi50% RH; ISO 527-2
 210 MPa30500 psiDAM; ISO 527-2
Elongation at Break 2.6 %2.6 %DAM; ISO 527-2
 5.8 %5.8 %50% RH; ISO 527-2
Tensile Modulus 10.0 GPa1450 ksi50% RH; ISO 527-2
 14.0 GPa2030 ksiDAM; ISO 527-2
Izod Impact, Notched (ISO)  17.0 kJ/m²
@Temperature 23.0 °C
8.09 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 180/1A
 24.0 kJ/m²
@Temperature 23.0 °C
11.4 ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 180/1A
 
Electrical PropertiesMetricEnglishComments
Comparative Tracking Index 575 V
@Thickness 3.00 mm
575 V
@Thickness 0.118 in
IEC 60112
 
Thermal PropertiesMetricEnglishComments
Melting Point 220 °C428 °FDAM; ISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 220 °C428 °FUnannealed; DAM; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 215 °C419 °FUnannealed; DAM; ISO 75-2/A
Flammability, UL94  HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
 HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 230 - 260 °C446 - 500 °FInjection
Middle Barrel Temperature 230 - 260 °C446 - 500 °FInjection
Front Barrel Temperature 230 - 260 °C446 - 500 °FInjection
Nozzle Temperature 230 - 260 °C446 - 500 °FInjection
Melt Temperature 230 - 260 °C446 - 500 °FInjection
Mold Temperature 80.0 - 90.0 °C176 - 194 °FInjection
Drying Temperature 80.0 - 90.0 °C176 - 194 °FInjection
Dry Time >= 3.00 hour>= 3.00 hourInjection
 
Descriptive Properties
AdditiveHeat Stabilizer
 Lubricant
AppearanceBlack
FeaturesChemical Resistant
 Gasoline Resistant
 General Purpose
 Good Flow
 High Heat Resistance
 Lubricated
FormsPellets
Processing MethodInjection Molding
RegionNorth America, Europe, Asia Pacific

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PASCE9278 / 287631

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.