MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Avient Edgetek® ES-30GF/000 Black Polyethersulfone (PESU)
Categories: Polymer; Thermoplastic; Polyethersulfone (PES)

Material Notes: Edgetek™ ES-30GF/000 Black XP120031

Information provided by PolyOne

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.59 g/cc1.59 g/ccASTM D792
Filler Content 30 %30 %Glass Fiber Reinforcement
Linear Mold Shrinkage, Flow 0.0010 - 0.0025 cm/cm0.0010 - 0.0025 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 131 MPa19000 psi5.1 mm/min; ASTM D638
Elongation at Break 4.0 %4.0 %Type I, 5.1 mm/min; ASTM D638
Tensile Modulus 7.58 GPa1100 ksiType I, 5.1 mm/min; ASTM D638
Flexural Strength 197 MPa28600 psiASTM D790
Flexural Modulus 6.89 GPa999 ksiASTM D790
Izod Impact, Notched 0.960 J/cm
@Thickness 6.35 mm,
Temperature 23.0 °C
1.80 ft-lb/in
@Thickness 0.250 in,
Temperature 73.4 °F
Injection Molded; ASTM D256A
 
Electrical PropertiesMetricEnglishComments
Surface Resistance 1.00e+14 ohm1.00e+14 ohmASTM D257
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 215 °C
@Thickness 3.18 mm
419 °F
@Thickness 0.125 in
Unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 205 °C
@Thickness 3.18 mm
401 °F
@Thickness 0.125 in
Unannealed; ASTM D648
 
Processing PropertiesMetricEnglishComments
Melt Temperature 340 - 380 °C644 - 716 °F
Mold Temperature 140 - 160 °C284 - 320 °F
Drying Temperature 150 - 160 °C302 - 320 °F
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hour
 
Descriptive Properties
FeaturesGeneral Purpose
 Good Chemical Resistance
 Good Dimensional Stability
 Good Strength
FormsPellets
Generic MaterialPESU
Generic NamePolyethersulfone (PESU)
Processing MethodInjection Molding
Regional AvailabilityAsia Pacific
UsesAutomotive Applications
 Consumer Applications
 General Purpose
 Industrial Applications

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
BASF Ultrason® E 2010 SW Q31 10088 PESU
BASF Ultrason® E 2010 MR SW 10111 PESU
BASF Ultrason® E 2010 HC PESU
BASF Ultrason® E 2010 G6 30% Glass Filled PES
Overview of materials for PBT + PET Blend, Glass Filled

PH0POL1120 / 145689

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.