MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Toyobo CoolPoly® D5522 LCP
Categories: Polymer; Thermoplastic; Liquid Crystal Polymer (LCP); Liquid Crystal Polymer (LCP), Unfilled

Material Notes: Product Description: CoolPoly D5522 offers thermal conductivity, excellent mechanical strength, surface appearance, low warpage, and excellent dimensional stability. Application of this grade is for a part with thin wall design in automotive and electronics. The D series is electrically non-conductive and can be used for its dielectric properties.

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Features: Low Warpage

Processing Method: Injection Molding

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.64 g/cc0.0592 lb/in³ISO 1183
Water Absorption 0.030 %0.030 %Equilibrium, 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0010 cm/cm0.0010 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.0060 cm/cm0.0060 in/inISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 143 MPa20700 psiISO 527-2/50
Elongation at Break 2.7 %2.7 %ISO 527-2/50
Tensile Modulus 14.0 GPa2030 ksiISO 527-1
Flexural Strength 160 MPa23200 psiISO 178
Flexural Modulus 13.0 GPa1890 ksiISO 178
Charpy Impact Unnotched 2.94 J/cm²14.0 ft-lb/in²ISO 179/1eU
Charpy Impact, Notched 1.01 J/cm²4.80 ft-lb/in²ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+13 ohm-cm>= 1.00e+13 ohm-cmIEC 62631-3-1
Surface Resistance >= 1.00e+14 ohm>= 1.00e+14 ohmIEC 62631-3-2
Dielectric Constant 3.63
@Frequency 1e+6 Hz
3.63
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 29.9 kV/mm760 kV/inIEC 60243-1
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 7.92 µm/m-°C4.40 µin/in-°FISO 11359-2
CTE, linear, Transverse to Flow 59.4 µm/m-°C33.0 µin/in-°FISO 11359-2
Specific Heat Capacity 1.38 J/g-°C0.330 BTU/lb-°FASTM E1461
Thermal Conductivity 0.605 W/m-K4.20 BTU-in/hr-ft²-°FThruplane; ASTM D1461
 0.994 W/m-K6.90 BTU-in/hr-ft²-°FCrossflow; ASTM D1461
 2.45 W/m-K17.0 BTU-in/hr-ft²-°FFlow; ASTM D1461
Melting Point 330 °C626 °FISO 11357-3
Deflection Temperature at 1.8 MPa (264 psi) 240 °C464 °FUnannealed; ISO 75-2/A
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 300 - 310 °C572 - 590 °F
Middle Barrel Temperature 310 - 320 °C590 - 608 °F
Front Barrel Temperature 320 - 330 °C608 - 626 °F
Nozzle Temperature 330 - 340 °C626 - 644 °F
Zone 4 330 - 340 °C626 - 644 °FInjection
Melt Temperature 330 - 345 °C626 - 653 °F
Mold Temperature 120 - 140 °C248 - 284 °F
Drying Temperature 150 °C302 °F
Dry Time 6.00 hour6.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PHCQ6270 / 310963

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.