MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

DuPont Mobility and Materials Minlon® 10B40HS1 BK061 PA66-MD40  (discontinued **)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 40% Mineral Filled

Material Notes: 40% Mineral Reinforced, Heat Stabilized, Polyamide 66

While this product line has been acquired by Celanese, this specific grade had been disconued while still a DuPont product so it is listed here as a discontinued DuPont product.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.51 g/cc0.0546 lb/in³DAM; ISO 1183
Linear Mold Shrinkage, Flow 0.0040 cm/cm0.0040 in/inDAM; ISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0090 cm/cm0.0090 in/inDAM; ISO 294-4, 2577
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 95.0 MPa13800 psiDAM; ISO 527-1/-2
Elongation at Break 2.5 %2.5 %DAM; ISO 527-1/-2
Tensile Modulus 10.0 GPa1450 ksiDAM; ISO 527-1/-2
Flexural Modulus 9.50 GPa1380 ksiDAM; ISO 178
Poissons Ratio 0.340.34DAM; ISO 527-1/-2
Izod Impact, Notched (ISO)  2.50 kJ/m²
@Temperature -40.0 °C
1.19 ft-lb/in²
@Temperature -40.0 °F
DAM; ISO 180/1A
 3.50 kJ/m²
@Temperature 23.0 °C
1.67 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 180/1A
Charpy Impact, Notched  0.200 J/cm²
@Temperature -40.0 °C
0.952 ft-lb/in²
@Temperature -40.0 °F
DAM; ISO 179/1eA
 0.300 J/cm²
@Temperature 23.0 °C
1.43 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 36.0 µm/m-°C20.0 µin/in-°FDAM; ISO 11359-1/-2
CTE, linear, Transverse to Flow 66.0 µm/m-°C36.7 µin/in-°FDAM; ISO 11359-1/-2
Melting Point 263 °C505 °F10°C/min; DAM; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 240 °C464 °FDAM; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 205 °C401 °FDAM; ISO 75-1/-2
Flammability, UL94 HB
@Thickness 0.710 mm
HB
@Thickness 0.0280 in
DAM; IEC 60695-11-10
Flame Spread <= 80.0 mm/min
@Thickness 1.00 mm
<= 3.15 in/min
@Thickness 0.0394 in
ISO 3795 (FMVSS 302)
 
Processing PropertiesMetricEnglishComments
Melt Temperature 295 °C563 °FInjection Optimum
 285 - 305 °C545 - 581 °FInjection
Mold Temperature 70.0 - 120 °C158 - 248 °FInjection
 100 °C212 °FInjection Optimum
Ejection Temperature 210 °C410 °F
Drying Temperature 80.0 °C176 °F
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hourDehumidified Dryer
Moisture Content 0.20 %0.20 %
Hold Pressure 50.0 - 100 MPa7250 - 14500 psi
 
Descriptive Properties
AdditivesRelease agent
Delivery formPellets
Drying Recommendedyes
FMVSS ClassBISO 3795 (FMVSS 302)
Hold pressure time (s/mm)3
Max. screw tangential speed (m/s)0.2DAM
Part Marking CodePA66-MD40ISO 11469
ProcessingInjection Molding
Regional AvailabilityNorth America
 South and Central America
Resin IdentificationPA66-MD40ISO 1043
Special characteristicsHeat stabilized or stable to heat

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Minlon® 10B40 NC010 PA66-MD40
Adell AH-38 Nylon 66, 40% Mineral Filled
Celanese Zytel® 70G33HS1L BK031 PA66-GF33
Celanese Zytel® 132F NC010 PA66
DuPont Mobility and Materials Minlon® EFE6096 GY090A PA66-IMD15

PDSX5239 / 197879

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.