MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

AISI Type 304L Stainless Steel, Annealed Bar, Longitudinal
Categories: Metal; Ferrous Metal; Heat Resisting; Stainless Steel; T 300 Series Stainless Steel

Material Notes: Austenitic Cr-Ni stainless steel. Better corrosion resistance than Type 302. High ductility, excellent drawing, forming, and spinning properties. Essentially non-magnetic, becomes slightly magnetic when cold worked. Low carbon content means less carbide precipitation in the heat-affected zone during welding and a lower susceptibility to intergranular corrosion. Applications include beer barrels, bellows, chemical equipment, coal hopper linings, cooling coils, cryogenic vessels, dairy equipment, evaporators, feedwater tubing, flexible metal hose, food processing equipment, hypodermic needles, nuclear vessels, oil well filter screens, refrigeration equipment, paper industry, pressure vessels, sanitary fittings, valves, shipping drums, spinning, still tubes, textile dyeing equipment, tubing.

Key Words: UNS S30403, SAE 30304L, DIN 1.4306, X2CrNi189, B.S. 304 S 12, PN 86020 (Poland), OOH18N10, ISO 4954 X2CrNi1810E, ISO 683/13 10, 18-8
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.00 g/cc0.289 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength  660 MPa
@Temperature 24.0 °C
95700 psi
@Temperature 75.2 °F
 1060 MPa
@Temperature -78.0 °C
154000 psi
@Temperature -108 °F
 1510 MPa
@Temperature -196 °C
219000 psi
@Temperature -321 °F
 1660 MPa
@Temperature -269 °C
241000 psi
@Temperature -452 °F
 1880 MPa
@Temperature -253 °C
273000 psi
@Temperature -423 °F
Tensile Strength, Yield  405 MPa
@Temperature 24.0 °C
58700 psi
@Temperature 75.2 °F
 435 MPa
@Temperature -78.0 °C
63100 psi
@Temperature -108 °F
 460 MPa
@Temperature -196 °C
66700 psi
@Temperature -321 °F
 525 MPa
@Temperature -253 °C
76100 psi
@Temperature -423 °F
 545 MPa
@Temperature -269 °C
79000 psi
@Temperature -452 °F
Elongation at Break  34 %
@Temperature -269 °C
34 %
@Temperature -452 °F
 42 %
@Temperature -253 °C
42 %
@Temperature -423 °F
 43 %
@Temperature -196 °C
43 %
@Temperature -321 °F
 70 %
@Temperature -78.0 °C
70 %
@Temperature -108 °F
 78 %
@Temperature 24.0 °C
78 %
@Temperature 75.2 °F
Reduction of Area  41 %
@Temperature -253 °C
41 %
@Temperature -423 °F
 56 %
@Temperature -269 °C
56 %
@Temperature -452 °F
 66 %
@Temperature -196 °C
66 %
@Temperature -321 °F
 74 %
@Temperature -78.0 °C
74 %
@Temperature -108 °F
 81 %
@Temperature 24.0 °C
81 %
@Temperature 75.2 °F
Modulus of Elasticity  190 GPa
@Temperature 24.0 °C
27600 ksi
@Temperature 75.2 °F
 200 GPa
@Temperature -269 °C
29000 ksi
@Temperature -452 °F
 205 GPa
@Temperature -196 °C
29700 ksi
@Temperature -321 °F
 
Electrical PropertiesMetricEnglishComments
Magnetic Permeability 1.0081.008at RT
 
Thermal PropertiesMetricEnglishComments
Specific Heat Capacity 0.500 J/g-°C0.120 BTU/lb-°FEstimate from similar stainless steels.
Thermal Conductivity 14.0 - 16.3 W/m-K97.0 - 113 BTU-in/hr-ft²-°F
Melting Point 1400 - 1450 °C2550 - 2640 °F
Solidus 1400 °C2550 °F
Liquidus 1450 °C2640 °F
Maximum Service Temperature, Air 870 °C1600 °FIntermittent
 925 °C1700 °FContinuous Service
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.030 %<= 0.030 %
Chromium, Cr 18 - 20 %18 - 20 %
Iron, Fe 64.9 - 74 %64.9 - 74 %as balance
Manganese, Mn <= 2.0 %<= 2.0 %
Nickel, Ni 8.0 - 12 %8.0 - 12 %
Phosphorus, P <= 0.045 %<= 0.045 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.030 %<= 0.030 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI Type 304L Stainless Steel
304 Stainless Steel
AK Steel 304L Austenitic Stainless steel
304 Stainless Steel (UNS S30400); Annealed Bar
AISI Type 316L Stainless Steel, annealed bar

MQ304Lc / 171854

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.