MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

Overview of materials for Silicone, Molded, Glass Fiber Filled
Categories: Polymer; Thermoset; Silicone; Silicone, Molded, Glass Fiber Filled

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Silicone, Molded, Glass Fiber Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.06 - 3.80 g/cc0.0383 - 0.137 lb/in³Average value: 1.42 g/cc Grade Count:323
Water Absorption 0.0200 - 0.450 %0.0200 - 0.450 %Average value: 0.181 % Grade Count:8
Thickness 12.7 - 25400 microns0.500 - 1000 milAverage value: 316 microns Grade Count:504
Linear Mold Shrinkage 0.00100 - 0.00800 cm/cm0.00100 - 0.00800 in/inAverage value: 0.00319 cm/cm Grade Count:7
Outgassing - Total Mass Loss 0.300 - 1.07 %0.300 - 1.07 %Average value: 0.678 % Grade Count:6
 0.340 - 0.340 %
@Temperature 218 - 218 °C
0.340 - 0.340 %
@Temperature 425 - 425 °F
Average value: 0.340 % Grade Count:1
 0.340 - 0.340 %
@Time 7200 - 7200 sec
0.340 - 0.340 %
@Time 2.00 - 2.00 hour
Average value: 0.340 % Grade Count:1
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 75.0 - 90.075.0 - 90.0Average value: 86.3 Grade Count:4
Hardness, Shore A 18.0 - 92.018.0 - 92.0Average value: 53.0 Grade Count:499
Tensile Strength, Ultimate 0.414 - 160 MPa60.0 - 23200 psiAverage value: 7.11 MPa Grade Count:508
Tensile Strength, Yield 3.45 - 62.1 MPa500 - 9000 psiAverage value: 25.0 MPa Grade Count:12
Elongation at Break 5.00 - 1150 %5.00 - 1150 %Average value: 394 % Grade Count:496
Elongation at Yield 31.0 - 38.0 %31.0 - 38.0 %Average value: 35.7 % Grade Count:3
Modulus of Elasticity 0.00159 - 14.0 GPa0.230 - 2030 ksiAverage value: 1.52 GPa Grade Count:15
Flexural Yield Strength 52.0 - 180 MPa7540 - 26100 psiAverage value: 94.1 MPa Grade Count:14
Flexural Modulus 8.00 - 16.0 GPa1160 - 2320 ksiAverage value: 12.6 GPa Grade Count:10
Compressive Yield Strength 40.0 - 331 MPa5800 - 48000 psiAverage value: 126 MPa Grade Count:13
Poissons Ratio 0.5000.500Average value: 0.500 Grade Count:27
Shear Modulus 0.000345 - 1.83 GPa0.0500 - 265 ksiAverage value: 0.454 GPa Grade Count:11
Shear Strength 0.965 - 20.0 MPa140 - 2900 psiAverage value: 4.48 MPa Grade Count:31
Adhesive Bond Strength 0.0103 - 150 MPa1.50 - 21800 psiAverage value: 3.62 MPa Grade Count:40
Izod Impact, Notched 0.220 - 3.78 J/cm0.412 - 7.08 ft-lb/inAverage value: 1.32 J/cm Grade Count:5
Charpy Impact Unnotched 0.400 - 2.50 J/cm²1.90 - 11.9 ft-lb/in²Average value: 1.38 J/cm² Grade Count:4
Tear Strength 4.91 - 51.9 kN/m28.0 - 296 pliAverage value: 17.4 kN/m Grade Count:181
Peel Strength 0.0877 - 7.05 kN/m0.500 - 40.2 pliAverage value: 1.46 kN/m Grade Count:353
Compression Set 25.0 - 49.0 %25.0 - 49.0 %Average value: 31.8 % Grade Count:4
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0500 - 1.00e+16 ohm-cm0.0500 - 1.00e+16 ohm-cmAverage value: 8.93e+14 ohm-cm Grade Count:7
Insulation Resistance 1.00e+8 - 1.00e+10 ohm1.00e+8 - 1.00e+10 ohmAverage value: 2.72e+9 ohm Grade Count:6
Dielectric Constant 3.20 - 6.913.20 - 6.91Average value: 4.75 Grade Count:35
Dielectric Strength 1.60 - 59.1 kV/mm40.6 - 1500 kV/inAverage value: 21.4 kV/mm Grade Count:454
 1.9685 - 7.00 kV/mm
@Temperature 90.0 - 90.0 °C
50.000 - 178 kV/in
@Temperature 194 - 194 °F
Average value: 4.48 kV/mm Grade Count:1
 1.9685 - 7.00 kV/mm
@Thickness 3.00 - 3.00 mm
50.000 - 178 kV/in
@Thickness 0.118 - 0.118 in
Average value: 4.48 kV/mm Grade Count:1
Dielectric Breakdown >= 25000 V
@Temperature 90.0 - 90.0 °C
>= 25000 V
@Temperature 194 - 194 °F
Average value: 31500 V Grade Count:2
 >= 30000 V
@Temperature 90.0 - 90.0 °C
>= 30000 V
@Temperature 194 - 194 °F
Average value: 31500 V Grade Count:2
 >= 30000 V
@Time 20.0 - 60.0 sec
>= 30000 V
@Time 0.00556 - 0.0167 hour
Average value: 31500 V Grade Count:2
Dissipation Factor 0.00150 - 0.07000.00150 - 0.0700Average value: 0.0109 Grade Count:35
Arc Resistance 180 - 240 sec180 - 240 secAverage value: 208 sec Grade Count:8
Comparative Tracking Index 300 - 450 V300 - 450 VAverage value: 390 V Grade Count:5
 
Thermal PropertiesMetricEnglishComments
CTE, linear 10.0 - 280 µm/m-°C5.56 - 156 µin/in-°FAverage value: 89.7 µm/m-°C Grade Count:29
 20.0 - 40.0 µm/m-°C
@Temperature 50.0 - 150 °C
11.1 - 22.2 µin/in-°F
@Temperature 122 - 302 °F
Average value: 30.0 µm/m-°C Grade Count:2
CTE, linear, Transverse to Flow 20.0 - 40.0 µm/m-°C11.1 - 22.2 µin/in-°FAverage value: 33.3 µm/m-°C Grade Count:3
Specific Heat Capacity 0.320 - 1.14 J/g-°C0.0765 - 0.272 BTU/lb-°FAverage value: 0.864 J/g-°C Grade Count:15
 0.820 - 0.920 J/g-°C
@Temperature 100 - 100 °C
0.196 - 0.220 BTU/lb-°F
@Temperature 212 - 212 °F
Average value: 0.842 J/g-°C Grade Count:13
Thermal Conductivity 0.0600 - 6.50 W/m-K0.416 - 45.1 BTU-in/hr-ft²-°FAverage value: 0.957 W/m-K Grade Count:33
 1.00 - 3.00 W/m-K
@Temperature 50.0 - 100 °C
6.94 - 20.8 BTU-in/hr-ft²-°F
@Temperature 122 - 212 °F
Average value: 1.94 W/m-K Grade Count:14
 1.50 - 4.69 W/m-K
@Temperature 50.0 - 50.0 °C
10.4 - 32.5 BTU-in/hr-ft²-°F
@Temperature 122 - 122 °F
Average value: 1.94 W/m-K Grade Count:4
 1.50 - 4.69 W/m-K
@Pressure 30.0 - 30.0 MPa
10.4 - 32.5 BTU-in/hr-ft²-°F
@Pressure 4350 - 4350 psi
Average value: 1.94 W/m-K Grade Count:4
Maximum Service Temperature, Air 95.6 - 300 °C204 - 572 °FAverage value: 228 °C Grade Count:414
Maximum Service Temperature, Inert 149 - 232 °C300 - 450 °FAverage value: 226 °C Grade Count:91
Deflection Temperature at 1.8 MPa (264 psi) 200 - 282 °C392 - 540 °FAverage value: 259 °C Grade Count:7
Minimum Service Temperature, Air -136 - -40.0 °C-212 - -40.0 °FAverage value: -58.5 °C Grade Count:491
Glass Transition Temp, Tg -120 - 118 °C-184 - 244 °FAverage value: -104 °C Grade Count:29
UL RTI, Electrical 150 - 220 °C302 - 428 °FAverage value: 211 °C Grade Count:127
UL RTI, Mechanical without Impact 150 - 220 °C302 - 428 °FAverage value: 203 °C Grade Count:127
Flammability, UL94 HB - V-0HB - V-0Grade Count:158
 
Processing PropertiesMetricEnglishComments
Processing Temperature 150 - 300 °C302 - 572 °FAverage value: 225 °C Grade Count:3
Cure Time 15.0 - 300 min
@Temperature 100 - 232 °C
0.250 - 5.00 hour
@Temperature 212 - 450 °F
Average value: 51.5 min Grade Count:412
 1.50 - 49.8 min
@Temperature 110 - 177 °C
0.0250 - 0.830 hour
@Temperature 230 - 350 °F
Average value: 51.5 min Grade Count:333
 1.50 - 49.8 min
@Pressure 0.0689 - 3.45 MPa
0.0250 - 0.830 hour
@Pressure 10.0 - 500 psi
Average value: 51.5 min Grade Count:333

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Silicone Rubber
Overview of materials for Silicone, RTV, Adhesive/Sealant Grade
Overview of materials for Styrenic Elastomer (TES)
Overview of materials for Thermoplastic Olefinic Elastomer (TPO)
Overview of materials for Silicone Elastomer, for Thermal Management

O5210 / 78477

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.