MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Ovako 34CrNiMo6 EN10083-3:2006 (ref) Steel, +QT
Categories: Metal; Ferrous Metal; Alloy Steel; AISI 4000 Series Steel

Material Notes: General Information: 34CrNiMo6 is a quenching and tempering steel with high strength, high toughness and good hardenability. Used for large axles, machine components, tools and high strength fasteners. The steel can be induction hardened and it is weldable under certain conditions. Through hardenability to appr. 100 mm diameter bar with oil quenching.
356D - Standard steel variant
356Q - IQ (isotropic quality) variant.
6499 - low sulphur variant of 34CrNiMo6
6507 - M-steel variant of 34CrNiMo6

IQ-SteelIQ-Steel® is an isotropic quality ultra clean steel optimized for high fatigue strength under multi axial loading.

Information provided by Ovako

Key Words: 34CrNiMo6M, 356, 356D, SS2541, MoCN315, MoCN315M, 1.6582, 35NCD6, 816M40, 817M40, 35NiCrMo6, SNCM447, 30Ch2N2MA, F.1272, 40NiCrMo7, 4337, 4340, 92541, VSQT34CrNiMo6, VSQT34CrNiMo6/700, VSQT34CrNiMo6/800, VSQT34CrNiMo6/900, Stål 2541, Steel 2541, EN24
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength  800 - 950 MPa
@Thickness 160.1 - 180 mm
116000 - 138000 psi
@Thickness 6.303 - 7.09 in
Round bar
 900 - 1100 MPa
@Thickness 100.1 - 160 mm
131000 - 160000 psi
@Thickness 3.941 - 6.30 in
Round bar
 1000 - 1200 MPa
@Thickness 40.1 - 100 mm
145000 - 174000 psi
@Thickness 1.58 - 3.94 in
Round bar
 1100 - 1300 MPa
@Thickness 16.1 - 40.0 mm
160000 - 189000 psi
@Thickness 0.634 - 1.57 in
Round bar
Tensile Strength, Yield  >= 600 MPa
@Thickness 160.1 - 180 mm
>= 87000 psi
@Thickness 6.303 - 7.09 in
Reh, Round bar
 >= 700 MPa
@Thickness 100.1 - 160 mm
>= 102000 psi
@Thickness 3.941 - 6.30 in
Reh, Round bar
 >= 800 MPa
@Thickness 40.1 - 100 mm
>= 116000 psi
@Thickness 1.58 - 3.94 in
Reh, Round bar
 >= 900 MPa
@Thickness 16.1 - 40.0 mm
>= 131000 psi
@Thickness 0.634 - 1.57 in
Reh, Round bar
Elongation at Break  10 %
@Thickness 16.1 - 40.0 mm
10 %
@Thickness 0.634 - 1.57 in
Round bar
 11 %
@Thickness 40.1 - 100 mm
11 %
@Thickness 1.58 - 3.94 in
Round bar
 12 %
@Thickness 100.1 - 160 mm
12 %
@Thickness 3.941 - 6.30 in
Round bar
 13 %
@Thickness 160.1 - 180 mm
13 %
@Thickness 6.303 - 7.09 in
Round bar
Reduction of Area  45 %
@Thickness 16.1 - 40.0 mm
45 %
@Thickness 0.634 - 1.57 in
Round bar
 50 %
@Thickness 40.1 - 100 mm
50 %
@Thickness 1.58 - 3.94 in
Round bar
 55 %
@Thickness 100.1 - 160 mm
55 %
@Thickness 3.941 - 6.30 in
Round bar
 55 %
@Thickness 160.1 - 180 mm
55 %
@Thickness 6.303 - 7.09 in
Round bar
Modulus of Elasticity 210 GPa30500 ksi
Poissons Ratio 0.300.30
Shear Modulus 80.0 GPa11600 ksi
Impact Test  45.0 J
@Thickness 16.1 - 40.0 mm,
Temperature 20.0 °C
33.2 ft-lb
@Thickness 0.634 - 1.57 in,
Temperature 68.0 °F
Round bar, long
 45.0 J
@Thickness 40.1 - 100 mm,
Temperature 20.0 °C
33.2 ft-lb
@Thickness 1.58 - 3.94 in,
Temperature 68.0 °F
Round bar, long
 45.0 J
@Thickness 100.1 - 160 mm,
Temperature 20.0 °C
33.2 ft-lb
@Thickness 3.941 - 6.30 in,
Temperature 68.0 °F
Round bar, long
 45.0 J
@Thickness 160.1 - 180 mm,
Temperature 20.0 °C
33.2 ft-lb
@Thickness 6.303 - 7.09 in,
Temperature 68.0 °F
Round bar, long
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000200 - 0.00000250 ohm-cm0.00000200 - 0.00000250 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 12.0 µm/m-°C
@Temperature 20.0 - 300 °C
6.67 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.460 - 0.480 J/g-°C
@Temperature 50.0 - 100 °C
0.110 - 0.115 BTU/lb-°F
@Temperature 122 - 212 °F
Thermal Conductivity 40.0 - 45.0 W/m-K278 - 312 BTU-in/hr-ft²-°FAmbient temperature
Transformation Temperature 315 °C599 °FMS
 725 °C1340 °FAC1
 785 °C1450 °FAC3
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.30 - 0.38 %0.30 - 0.38 %
Chromium, Cr 1.3 - 1.7 %1.3 - 1.7 %
Iron, Fe 94.66 - 96.45 %94.66 - 96.45 %As Balance
Manganese, Mn 0.50 - 0.80 %0.50 - 0.80 %
Molybdenum, Mo 0.15 - 0.30 %0.15 - 0.30 %
Nickel, Ni 1.3 - 1.7 %1.3 - 1.7 %
Phosphorus, P <= 0.025 %<= 0.025 %
Silicon, Si <= 0.40 %<= 0.40 %
Sulfur, S <= 0.035 %<= 0.035 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI 4340 Steel, oil quenched 845°C, 425°C (800°F) temper
ATI Allvac® Vasco® 4340 Specialty Steel, Heat Treatment: 899°C (1650°F) Q+T
Ovako 42NiSiCrMo8-7-3* 497Q Steel, Quenching
AISI 4340 Steel, oil quenched 830°C (1525°F), 540°C (1000°F) temper, nitrided
AISI 4340 Steel, oil quenched 855°C (1570°F), 230°C (450°F) temper for 4 hrs.

NOVAKO269 / 234568

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.