MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

BASF 3D Ultrafuse® PLA Fused Fillament
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoplastic; Polylactic Acid (PLA) Biopolymer

Material Notes: Components: Polylactic acid based filament for Fused Filament Fabrication.

Product Description: PLA is one of the most used materials for 3D printing. Ultrafuse PLA is available in a wide range of colors. The glossy feel often attracts those who print display models or items for household use. Many appreciate the plant-based origin of this material. When properly cooled, PLA has a high maximum printing speed and sharp printed corners. Combining this with low warping of the print makes it a popular plastic for home printers, hobbyists, prototyping and schools.

Information provided by BASF

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.248 g/cc0.04509 lb/in³Printed Part; ISO 1183-1
Melt Flow 26.4576 g/10 min
@Load 5.00 kg,
Temperature 220 °C
26.4576 g/10 min
@Load 11.0 lb,
Temperature 428 °F
ISO 1133
Storage Temperature 15.0 - 25.0 °C59.0 - 77.0 °F
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 21.2 MPa3070 psiZX: Upright; ISO 527
 34.7 MPa5030 psiXY: Flat; ISO 527
Elongation at Break 1.2 %1.2 %ZX: Upright; ISO 527
 4.2 %4.2 %XY: Flat; ISO 527
Modulus of Elasticity 2.131 GPa309.1 ksiYoung's, ZX: Upright; ISO 527
 2.308 GPa334.8 ksiYoung's, XY: Flat; ISO 527
Flexural Strength 54.9 MPa7960 psiZX: Upright; ISO 178
 98.0 MPa14200 psiXY: Flat; ISO 178
 105 MPa15200 psiXZ: On its edge; ISO 178
Flexural Modulus 1.708 GPa247.7 ksiXZ: On its edge; ISO 178
 1.715 GPa248.7 ksiZX: Upright; ISO 178
 1.86 GPa270 ksiXY: Flat; ISO 178
Flexural Strain at Break 1.9 %1.9 %ZX: Upright; ISO 178
 4.2 %4.2 %XZ: On its edge; ISO 178
 4.8 %4.8 %XY: Flat; ISO 178
Izod Impact, Notched (ISO) 1.60 kJ/m²0.761 ft-lb/in²ZX: Upright; ISO 180
 2.10 kJ/m²0.999 ft-lb/in²XZ: On its edge; ISO 180
 3.30 kJ/m²1.57 ft-lb/in²XY: Flat; ISO 180
Izod Impact, Unnotched (ISO) 4.70 kJ/m²2.24 ft-lb/in²ZX: Upright; ISO 180
 9.60 kJ/m²4.57 ft-lb/in²XZ: On its edge; ISO 180
 11.0 kJ/m²5.23 ft-lb/in²XY: Flat; ISO 180
Charpy Impact Unnotched 0.430 J/cm²2.05 ft-lb/in²ZX: Upright; ISO 179-2
 1.32 J/cm²6.28 ft-lb/in²XY: Flat; ISO 179-2
 1.43 J/cm²6.80 ft-lb/in²XZ: On its edge; ISO 179-2
Charpy Impact, Notched 0.170 J/cm²0.809 ft-lb/in²ZX: Upright; ISO 179-2
 0.190 J/cm²0.904 ft-lb/in²XZ: On its edge; ISO 179-2
 0.250 J/cm²1.19 ft-lb/in²XY: Flat; ISO 179-2
 
Thermal PropertiesMetricEnglishComments
Melting Point 151 °C304 °FISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 65.0 °C149 °FISO 75-2
Deflection Temperature at 1.8 MPa (264 psi) 55.0 °C131 °FISO 75-2
Glass Transition Temp, Tg 61.0 °C142 °FISO 11357-2
 
Processing PropertiesMetricEnglishComments
Processing Temperature 50.0 - 70.0 °C122 - 158 °FBed, Bed Material: Glass
Nozzle Temperature 210 - 230 °C410 - 446 °F
Shelf Life 12.0 Month12.0 Month
 
Descriptive Properties
Nozzle Diameter=0.4 mm
Print speed40-80 mm/s

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PBASF3D000 / 312241

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.