MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AISI Type A9 Tool Steel
Categories: Metal; Ferrous Metal; Tool Steel; Air-Hardening Steel; Cold Work Steel

Material Notes: Higher shock resistance, but lower wear resistance than other air-hardened tool steels. High hardenability, high degree of dimensional stability in heat treatment, good wear resistance, fatigue life, toughness, and deep hardening qualities. Applications include cold forming, blanking and bending dies, forming rolls, drill bushings, knurling tools, master dies and gauges.

Key Words: UNS T30109, ASTM A681, FED QQ-T-570
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.78 g/cc0.281 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Knoop 662662Converted from Rockwell C hardness.
Hardness, Rockwell C 5757tempered at 500°C
Hardness, Vickers 641641
Tensile Strength, Ultimate 2200 MPa319000 psitempered at 500°C
Tensile Strength, Yield 1780 MPa258000 psitempered at 500°C
Elongation at Break 5.0 %5.0 %in 50 mm; tempered at 500°C
Izod Impact 18.0 J13.3 ft-lbsmooth bar; tempered at 500°C
 
Thermal PropertiesMetricEnglishComments
CTE, linear 12.0 µm/m-°C6.67 µin/in-°F
 
Processing PropertiesMetricEnglishComments
Processing Temperature 510 - 620 °C950 - 1150 °FTempering Temperature
 980 - 1025 °C1800 - 1877 °FHardening Temperature
Annealing Temperature 845 - 870 °C1550 - 1600 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.45 - 0.55 %0.45 - 0.55 %
Chromium, Cr 4.75 - 5.5 %4.75 - 5.5 %
Iron, Fe 87.3 - 90.5 %87.3 - 90.5 %As Balance
Manganese, Mn <= 0.50 %<= 0.50 %
Molybdenum, Mo 1.3 - 1.8 %1.3 - 1.8 %
Nickel, Ni 1.25 - 1.75 %1.25 - 1.75 %
Phosphorus, P <= 0.030 %<= 0.030 %
Silicon, Si 0.95 - 1.15 %0.95 - 1.15 %
Sulfur, S <= 0.030 %<= 0.030 %
Vanadium, V 0.80 - 1.4 %0.80 - 1.4 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI Type A8 Tool Steel
AISI Type A2 Tool Steel
AISI Type A3 Tool Steel
AISI Type A10 Tool Steel
AISI Type A4 Tool Steel

MSTA9 / 14250

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.