MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

305 Stainless Steel, Hot finished and annealed bar, forgings
Categories: Metal; Ferrous Metal; Stainless Steel; T 300 Series Stainless Steel

Material Notes: Same corrosion resistance and Type 302, but much lower rate of work hardening. Excellent cold formability, good free spinning and cold heading properties, recommended for severe cold drawing. Applications include electronic parts and other drawn applications.

Key Words: UNS S30500, ASTM A 473 A473
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.00 g/cc0.289 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 515 MPa74700 psi
Tensile Strength, Yield 205 MPa29700 psi
Elongation at Break 30 %30 %
Reduction of Area 40 %40 %
Modulus of Elasticity 193 GPa28000 ksi
Shear Modulus 86.0 GPa12500 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000720 ohm-cm
@Temperature 20.0 °C
0.0000720 ohm-cm
@Temperature 68.0 °F
Magnetic Permeability 1.0081.008at RT
 
Thermal PropertiesMetricEnglishComments
CTE, linear  17.3 µm/m-°C
@Temperature 0.000 - 100 °C
9.61 µin/in-°F
@Temperature 32.0 - 212 °F
 17.8 µm/m-°C
@Temperature 0.000 - 315 °C
9.89 µin/in-°F
@Temperature 32.0 - 599 °F
 18.4 µm/m-°C
@Temperature 0.000 - 540 °C
10.2 µin/in-°F
@Temperature 32.0 - 1000 °F
 18.7 µm/m-°C
@Temperature 0.000 - 650 °C
10.4 µin/in-°F
@Temperature 32.0 - 1200 °F
Specific Heat Capacity 0.500 J/g-°C
@Temperature 0.000 - 100 °C
0.120 BTU/lb-°F
@Temperature 32.0 - 212 °F
Thermal Conductivity  16.3 W/m-K
@Temperature 100 °C
113 BTU-in/hr-ft²-°F
@Temperature 212 °F
 21.5 W/m-K
@Temperature 500 °C
149 BTU-in/hr-ft²-°F
@Temperature 932 °F
Melting Point 1400 - 1455 °C2550 - 2651 °F
Solidus 1400 °C2550 °F
Liquidus 1455 °C2651 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.12 %<= 0.12 %
Chromium, Cr 18 %18 %
Iron, Fe 67 %67 %
Manganese, Mn <= 2.0 %<= 2.0 %
Nickel, Ni 12 %12 %
Phosphorus, P <= 0.045 %<= 0.045 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.030 %<= 0.030 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
303 MA Stainless Steel, in bar, annealed
305 Stainless Steel, annealed, sheet
303 SE Stainless Steel, cold drawn, bar
AISI 4817 Steel
AISI 8620 Steel, annealed 13 mm (0.5 in.) round

MQ305M / 171828

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.