MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Dioshy E963D-GS Thermoplastic Polyester Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyester TPE

Material Notes: Thermoplastic polyester elastomer (TPEE), high performance engineering elastomers; hardness range Shore D 30 ~ Shore D 72.

Features:

  • Excellent anti-fatigue and tough; suitable to engineering mechanical products.
  • Very good oil resistance and chemical resistance; good compression set; white color.
  • Good processing ability, suitable to mostly thermoplastic procedures.
  • Green material, passed heavy metal regulation, RoHS and EACH –SVHC .

      Information provided by DIOSHY CO., LTD

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.233 g/cc1.233 g/ccJIS-K6301
Melt Flow 37.98 g/10 min
@Load 2.16 kg,
Temperature 230 °C
37.98 g/10 min
@Load 4.76 lb,
Temperature 446 °F
JIS-K7210
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 6363JIS-K6301
Tensile Strength 31.4 MPa4550 psiJIS-K6310
Elongation at Break 541 %541 %JIS-K6310
100% Modulus 19.3 MPa2800 psiJIS-K6310
300% Modulus 6.37 MPa925 psiJIS-K6310
Tear Strength 2527 kN/m14430 pliJIS-K6310-B
Compression Set 21 %
@Temperature 23.0 °C,
Time 79200 sec
21 %
@Temperature 73.4 °F,
Time 22.0 hour
JIS-K6301
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+13 ohm-cm>= 1.00e+13 ohm-cm
Dielectric Strength 26.0 kV/mm660 kV/in
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 190 - 200 °C374 - 392 °FExtrusion
 195 - 205 °C383 - 401 °FInjection
Middle Barrel Temperature 200 - 210 °C392 - 410 °FExtrusion
 205 - 215 °C401 - 419 °FInjection
Front Barrel Temperature 200 - 210 °C392 - 410 °FExtrusion
 205 - 215 °C401 - 419 °FInjection
Nozzle Temperature 225 - 235 °C437 - 455 °FInjection
Die Temperature 215 - 225 °C419 - 437 °FExtrusion
Drying Temperature 100 °C212 °F
Dry Time 2.00 hour2.00 hour
 
Descriptive Properties
ColorWhite
TPEE TypeTPC-ET

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PDIOSH047 / 294657

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.