MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

SEKISUI SPI ALLEN® 4225F High Impact ABS Sheet
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Impact Grade, Molded; Acrylonitrile Butadiene Styrene (ABS), Sheet

Material Notes: ALLEN® 4225F is a general purpose ABS that has high impact strength and a good cost to performance ratio to other materials like stainless steel, and other thermoplastics.

ALLEN® 4225F has been tested under laboratory conditions and has achieved a UL94 HB rating at 0.060 in (1.52mm) and above and meets the requirements of Federal Motor Vehicle Safety Standard No. 302 (FMVSS 302) and US Food And Drug Administration 21 CFR 181.32 (Acrylonitrile copolymers and resins).

Suggested Application:

  • Mechanical covers & housings
  • Beverages dispensers
  • Ice bins
  • Food equipment
Features:
  • Custom color matching
  • Good forming properties
  • Edge trim easily used in future orders
  • High gloss, high impact
  • Excellent low temperature performance
  • FDA 21 CFR 181.32 compliant

Information provided by SEKISUI KYDEX, LLC.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.06 g/cc1.06 g/ccASTM D792
Water Absorption 0.280 %
@Time 86400 sec
0.280 %
@Time 24.0 hour
ASTM D570
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 98.098.0ASTM D785
Tensile Strength 36.7 MPa5320 psiASTM D638
Tensile Modulus 2.02 GPa293 ksiASTM D638
Flexural Strength 61.5 MPa
@Strain 5.00 %
8920 psi
@Strain 5.00 %
ASTM D790
Flexural Modulus 2.12 GPa307 ksiASTM D790
Compressive Strength 49.6 MPa7190 psiASTM D695
Bearing Yield Strength <= 358.8 MPa<= 52040 psiASTM D953
 180.6 MPa
@Strain 4.00 %
26190 psi
@Strain 4.00 %
ASTM D953
Shear Strength 40.1 MPa5820 psiASTM D732
Izod Impact, Notched 4.32 J/cm8.09 ft-lb/inASTM D256
Gardner Impact 24.0 J17.7 ft-lbDrop Dart Impact, GE; ASTM D5420
 
Electrical PropertiesMetricEnglishComments
Dielectric Strength 17.4 kV/mm442 kV/inoil; ASTM D149
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 90.1 µm/m-°C50.1 µin/in-°FASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 104 °C219 °Fannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 99.9 °C212 °Fannealed; ASTM D648
Flammability, UL94 HB
@Thickness 1.52 mm
HB
@Thickness 0.0598 in

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSEKIS545 / 325285

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.