MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Celanese Ateva® 1061 Ethylene Vinyl Acetate Copolymer Film  (discontinued **)
Categories: Polymer; Film; Thermoplastic; Ethylene Vinyl Acetate; Ethylene Vinyl Acetate Copolymer (EVA), Film Grade

Material Notes: Ateva® 1061 resin is suitable for laminating and co-extrusion applications with excellent sealability, opticals and strength. This EVA resin may be safely used as articles or components of articles intended for uses in contact with food as provided in FDA regulation 21 CFR 177.1350 - Ethylene-vinyl acetate copolymers, subject to extraction limitations on the finished food-contact article as specified in that regulation. Properties listed are for a film produced on a three layer co-extrusion with a 76 mm die, at a stock temperature of 210°C. Additives:

Applications: Flexible Packaging

Information provided by Celanese Corporation.

Key Words: laminating and co-extrusion applications with excellent sealability, opticals and strength
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.925 g/cc0.0334 lb/in³ASTM D1505; ASTM D1928 Proc A
Vinyl Acetate Content 6.0 %6.0 %AT Plastics PTM-39
Thickness 31.0 microns1.22 mil
Melt Flow 1.8 g/10 min
@Load 2.16 kg,
Temperature 190 °C
1.8 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 10.0 MPa1450 psiMethod A (500 mm/min); ASTM D882
Film Tensile Strength at Yield, TD 9.00 MPa1310 psiMethod A (500 mm/min); ASTM D882
Film Elongation at Break, MD 440 %440 %Method A (500 mm/min); ASTM D882
Film Elongation at Break, TD 560 %560 %Method A (500 mm/min); ASTM D882
Secant Modulus, MD 0.120 GPa17.4 ksi1% Secant Modulus; ASTM D882
Secant Modulus, TD 0.115 GPa16.7 ksi1% Secant Modulus; ASTM D882
Dart Drop 2.80 g/micron71.1 g/milf50; ASTM D1709
Film Tensile Strength at Break, MD 29.0 MPa4210 psiMethod A (500 mm/min); ASTM D882
Film Tensile Strength at Break, TD 19.0 MPa2760 psiMethod A (500 mm/min); ASTM D882
 
Thermal PropertiesMetricEnglishComments
Melting Point 104 °C219 °FDSC; ASTM D3417
Vicat Softening Point 92.0 °C198 °FASTM D1525
 
Optical PropertiesMetricEnglishComments
Haze 4.0 %4.0 %ASTM D1003
Gloss 68 %68 %45°; ASTM D2457
 
Processing PropertiesMetricEnglishComments
Processing Temperature 160 - 210 °C320 - 410 °F
Blow-up Ratio (BUR) 2.02.0
 
Compliance PropertiesMetricEnglishComments
FDA YesYesSee notes for details.

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Braskem CN8092 EVA Molding Copolymer
Arkema EVATANE® 33-25 Copolymer Ethylene - Vinyl Acetate
Arkema EVATANE® 20-20 Copolymer Ethylene - Vinyl Acetate
Petroquimica Triunfo Tritheva® PN 2021 EVA Copolymer
Braskem TN2020 EVA General Film Copolymer

PATEVB34 / 25990

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.