MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Abatron AboCast 8110-2/AboCure 8110-3 Flexible Epoxy
Categories: Polymer; Adhesive; Thermoset; Epoxy; Epoxy Adhesive, Flexible

Material Notes: This epoxy system can achieve flexibility and plasticity without sacrificing adhesive, electrical, structural, and other properties. This compound is a clear (unfilled) basic formulation. Its applications include: bonding, laminating, casting, embedding, electrical potting, impregnating, coating, etc. It can be supplied in several variations to modify viscosity, reaction rate, color, most physical and chemical properties, and with many fillers to meet most requirements.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Water Absorption  4.5 %
@Time 2.59e+6 sec
4.5 %
@Time 720 hour
immersion; cured 30 days @ 25°C
 4.6 %
@Time 2.59e+6 sec
4.6 %
@Time 720 hour
immersion; cured 7 days @ 25°C
 4.6 %
@Time 7200 sec
4.6 %
@Time 2.00 hour
boil; cured 2 hours @ 93°C
 4.7 %
@Time 2.59e+6 sec
4.7 %
@Time 720 hour
immersion; cured 90 days @ 25°C
Viscosity 1050 cP1050 cP
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D  15
@Temperature 75.0 °C
15
@Temperature 167 °F
cured 7 days @ 25°C
 75
@Temperature 25.0 °C
75
@Temperature 77.0 °F
cured 2 hrs. @ 93°C
 75
@Temperature 25.0 °C
75
@Temperature 77.0 °F
cured 7 days @ 25°C
 85
@Temperature -60.0 °C
85
@Temperature -76.0 °F
cured 7 days @ 25°C
 85
@Temperature 0.000 °C
85
@Temperature 32.0 °F
cured 7 days @ 25°C
 90
@Temperature -60.0 °C
90
@Temperature -76.0 °F
cured 2 hrs. @ 93°C
 90
@Temperature 0.000 °C
90
@Temperature 32.0 °F
cured 2 hrs. @ 93°C
Tensile Strength, Ultimate 7.93 MPa1150 psicured 30 days @ 25°C
 8.00 MPa1160 psicured 7 days @ 25°C
 13.2 MPa1910 psicured 90 days @ 25°C
 15.2 MPa2200 psicured 2 hours @ 93°C
Elongation at Break 125 %125 %cured 30 days @ 25°C
 130 %130 %cured 2 hours @ 93°C
 160 %160 %cured 7 days @ 25°C
Shear Strength  8.96 MPa
@Temperature 0.000 °C
1300 psi
@Temperature 32.0 °F
Tensile, Al/Al lap joint; cured 7 days @ 25°C
 12.3 MPa
@Temperature 25.0 °C
1780 psi
@Temperature 77.0 °F
Tensile, Al/Al lap joint; cured 90 days @ 25°C
 13.82 MPa
@Temperature 25.0 °C
2005 psi
@Temperature 77.0 °F
Tensile, Al/Al lap joint; cured 30 days @ 25°C
 15.55 MPa
@Temperature 25.0 °C
2255 psi
@Temperature 77.0 °F
Tensile, Al/Al lap joint; cured 2 hours @ 93°C
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity  3.50e+11 ohm-cm
@Temperature 25.0 °C
3.50e+11 ohm-cm
@Temperature 77.0 °F
cured 30 days @ 25°C
 5.30e+11 ohm-cm
@Temperature 25.0 °C
5.30e+11 ohm-cm
@Temperature 77.0 °F
cured 90 days @ 25°C
 7.50e+11 ohm-cm
@Temperature 25.0 °C
7.50e+11 ohm-cm
@Temperature 77.0 °F
cured 2 hours @ 93°C
 1.10e+12 ohm-cm
@Temperature 25.0 °C
1.10e+12 ohm-cm
@Temperature 77.0 °F
cured 7 days @ 25°C
 
Processing PropertiesMetricEnglishComments
Pot Life 20 min
@Temperature 25.0 °C
20 min
@Temperature 77.0 °F
200 g
 
Descriptive Properties
Parts by Weight (pbw)100AboCast 8110-2
 13AboCure 8110-3

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
MarkeTech AO 98 Aluminum Oxide Ceramic Substrate, 98% Purity
MarkeTech AO 95 Aluminum Oxide Ceramic Substrate, 95% Purity
MarkeTech AN 120 Aluminum Nitride Ceramic Substrate, 98% Purity
AISI 9255 Steel, normalized at 900°C (1650°F)
Abatron AboCast 8110-5/AboCure 8110-1 Flexible Epoxy

PABC866 / 107850

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.