MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

A. Schulman PP 1102-01 Polypropylene General Purpose, Molding Grade Polypropylene
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Molded

Material Notes: Description

Polypropylene PP 1102-01 is a general purpose, molding grade with UL 94 HB approval for use in large and thin wall applications.
Application

Polypropylene PP 1102-01 meets FDA Regulation 21 CFR 177.1520 for all food contact applications.
Information provided by A. Schulman.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.900 g/cc0.900 g/ccASTM D792
Melt Flow 12 g/10 min12 g/10 minASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 9595ASTM D785
Tensile Strength, Yield 31.7 MPa4600 psiASTM D638
Elongation at Break 8.0 %8.0 %ASTM D638
Flexural Modulus 1.31 GPa190 ksiASTM D790
Izod Impact, Notched 0.267 J/cm0.500 ft-lb/inASTM D256
 
Thermal PropertiesMetricEnglishComments
Melting Point 160 °C320 °FDSC
Deflection Temperature at 0.46 MPa (66 psi) 102 °C216 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 62.0 °C144 °FASTM D648
 
Compliance PropertiesMetricEnglishComments
FDA YesYesSee notes for details.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
A. Schulman POLYFORT™ FPP 1697HU High Flow Fortified Polypropylene
Ampco Metal AMPCO® 673 Manganese Bronze
Celanese Hostaform® XGC25 POM, 25% Glass Reinforced
High-Leaded Tin Bronze, UNS C93200, Copper Casting Alloy, Bearing Bronze SAE 660
Manganese Brass, UNS C67300

PASHU207 / 25171

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.