MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Akro-Plastic Akromid® S3 GF 50 1 (3533) PA 6.10 Dry, 50% Glass Filled
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 610 (PA610); Nylon 610, Glass Reinforced

Material Notes: A characteristic property of AKROMID® S (PA 6.10) is that it has a renewable-resource content of up to 70%. The plant-based raw material used is sebacic acid, synthesized from castor oil which is obtained from the seeds of Ricinus communis, the castor oil plant. From a technical standpoint, AKROMID® S closes the gap between PA 6/PA 6.6 and PA 12. It is characterized by significantly lower moisture absorption compared to PA 6 and PA 6.6. At 23 °C and 50% relative humidity, typical values for these product types are 3% and 2.8%, respectively. With a value of approximately 1.4%, PA 6.10 absorbs just half as much moisture and can therefore be used as an engineering material in applications requiring a high dimensional consistency. It exhibits excellent cold impact resistance. Other outstanding characteristics include very good chemical resistance due to the structure of the polymer and high hydrolysis resistance, although it can be processed like all common polyamides. The materials from the PA 6.10 product family are further characterized by exceptional dimensional stability, good surface resistance, good abrasion resistance and wear behavior, and an improved carbon footprint. This is due to the fact that the plant-based raw materials have already removed CO2 from the environment during their growth phase. The product portfolio currently comprises one non reinforced variant and several reinforced variants with a glass-fiber content ranging from 15% to 50 %. Unlike certain materials used in the packaging industry, the material is not biodegradable.

Applications:

    Automotive Sector
  • Connectors and housings
  • Non-return valves
  • Power steering-fluid reservoirs
  • Corrugated tubing and fluid pipes
    Machine Construction and Tool-Building
  • Gears
  • Door handles and fittings
  • Office equipment, housings, functional parts, amongst others
  • Connectors and plugs
  • Power tools
    Sports and Leisure
  • Components in high-end garden tools
  • Bicycle accessories
  • Sail-boat accessories
  • Winter sports accessories

    Information from Akro-Plastic

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.51 g/cc
@Temperature 23.0 °C
0.0546 lb/in³
@Temperature 73.4 °F
ISO 1183
Filler Content 50 %50 %ISO 1172
Moisture Absorption 0.90 %
@Temperature 70.0 °C
0.90 %
@Temperature 158 °F
62% r.h.; ISO 62
Water Absorption at Saturation  0.35 %
@Temperature 25.0 °C,
Treatment Temp. 70.0 °C
0.35 %
@Temperature 77.0 °F,
Treatment Temp. 158 °F
62% rel. humidity
 0.40 %
@Temperature 50.0 °C,
Treatment Temp. 70.0 °C
0.40 %
@Temperature 122 °F,
Treatment Temp. 158 °F
62% rel. humidity
 0.60 %
@Treatment Temp. 70.0 °C,
Temperature 145 °C
0.60 %
@Treatment Temp. 158 °F,
Temperature 293 °F
62% rel. humidity
 0.70 %
@Treatment Temp. 70.0 °C,
Temperature 310 °C
0.70 %
@Treatment Temp. 158 °F,
Temperature 590 °F
62% rel. humidity
 0.70 %
@Treatment Temp. 70.0 °C,
Temperature 335 °C
0.70 %
@Treatment Temp. 158 °F,
Temperature 635 °F
62% rel. humidity
 0.75 %
@Treatment Temp. 70.0 °C,
Temperature 220 °C
0.75 %
@Treatment Temp. 158 °F,
Temperature 428 °F
62% rel. humidity
Linear Mold Shrinkage, Flow 0.0030 cm/cm0.0030 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.010 cm/cm0.010 in/inISO 294-4
Spiral Flow 35.0 cm13.8 inAKRO
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 230 MPa33400 psiH 961/30; ISO 2039-1
Tensile Strength at Break 200 MPa29000 psi5 [mm/min]; ISO 527-1/2
Elongation at Break 3.5 %3.5 %5 [mm/min]; ISO 527-1/2
Tensile Modulus 14.5 GPa2100 ksi1[mm/min]; ISO 527-1/2
 10.5 GPa
@Treatment Temp. 70.0 °C,
Time 1.22e+6 sec
1520 ksi
@Treatment Temp. 158 °F,
Time 340 hour
62% rel. humidity
 10.8 GPa
@Treatment Temp. 70.0 °C,
Time 1.15e+6 sec
1570 ksi
@Treatment Temp. 158 °F,
Time 320 hour
62% rel. humidity
 11.0 GPa
@Treatment Temp. 70.0 °C,
Time 936000 sec
1600 ksi
@Treatment Temp. 158 °F,
Time 260 hour
62% rel. humidity
 11.5 GPa
@Treatment Temp. 70.0 °C,
Time 522000 sec
1670 ksi
@Treatment Temp. 158 °F,
Time 145 hour
62% rel. humidity
 12.4 GPa
@Treatment Temp. 70.0 °C,
Time 180000 sec
1800 ksi
@Treatment Temp. 158 °F,
Time 50.0 hour
62% rel. humidity
 12.5 GPa
@Treatment Temp. 70.0 °C,
Time 90000 sec
1810 ksi
@Treatment Temp. 158 °F,
Time 25.0 hour
62% rel. humidity
Flexural Strength 310 MPa45000 psi2 [mm/min]; ISO 178
Flexural Modulus 13.8 GPa2000 ksi2 [mm/min]; ISO 178
Flexural Strain at Break 3.6 %3.6 %2 [mm/min]; ISO 178
Charpy Impact Unnotched  10.0 J/cm²
@Temperature 23.0 °C
47.6 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
 10.5 J/cm²
@Temperature -30.0 °C
50.0 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched  1.60 J/cm²
@Temperature -30.0 °C
7.61 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 2.00 J/cm²
@Temperature 23.0 °C
9.52 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Melting Point 220 °C428 °FISO 11357-1, DSC,10 [K/min]
Deflection Temperature at 1.8 MPa (264 psi) 205 °C401 °FHDT/A; ISO 75-1/2
Deflection Temperature at 8.0 MPa 170 °C338 °FHDT/C; ISO 75-1/2
Flammability, UL94 HB
@Thickness 0.800 mm
HB
@Thickness 0.0315 in
 
Processing PropertiesMetricEnglishComments
Feed Temperature 60.0 - 80.0 °C140 - 176 °F
Nozzle Temperature 240 - 295 °C464 - 563 °F
Zone 1 220 - 300 °C428 - 572 °F
Zone 2 220 - 300 °C428 - 572 °F
Zone 3 220 - 300 °C428 - 572 °F
Zone 4 220 - 300 °C428 - 572 °F
Melt Temperature 260 - 310 °C500 - 590 °F
Mold Temperature 70.0 - 100 °C158 - 212 °F
Drying Temperature 80.0 °C176 °F
Dry Time <= 4 hour<= 4 hour
Hold Pressure 30.0 - 80.0 MPa4350 - 11600 psi
Back Pressure 5.00 - 15.0 MPa725 - 2180 psi
 
Descriptive Properties
Rate acc. FMVSS 302 (<100/min)Passed
Rate acc. FMVSS 302,(<100/min)FMVSS 302, >1 [mm] Thickness

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
A. Schulman ComAlloy Lubrilon® 646 Nylon 6/12, Carbon Fiber/PTFE Reinforced
Akro-Plastic Akromid® S3 GF 23 1 (2917) PA 6.10 Dry, 23% Glass Filled
Akro-Plastic Akromid® S3 GF 30 1 (3222) PA 6.10 Conditioned, 30% Glass Filled
Evonik Trogamid® T5002 Nylon 6-3 Compound
3M Nextel™ CF-40 Woven Fabric 550

PAKRO051 / 126831

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.