MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Titanium Beta III (Ti-11.5Mo-6Zr-4.5Sn; Grade 10), ST 775°C, Aged 550°C
Categories: Metal; Nonferrous Metal; Titanium Alloy; Beta Titanium Alloy

Material Notes: Microstructure: Beta alloy, can be aged without forming intermetallic compounds.

Characteristics: High strength, good hardenability, good resistance to stress corrosion, good cold-formability.

Applications: Aircraft fasteners and sheet metal parts, to a lesser extent - plate and forging applications.

5 other heat treatments of this alloy are in MatWeb.

Key Words: Ti-11.5Mo-6Zr-4.5Sn; UNS R58030; Beta 3
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 5.06 g/cc0.183 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Vickers 325325
Tensile Strength, Ultimate 1255 MPa182000 psi
Tensile Strength, Yield 1180 MPa171000 psi
Elongation at Break 5.0 %5.0 %
Reduction of Area 12 %12 %
Modulus of Elasticity 108 GPa15700 ksiSample STA 720°C/495°C
Compressive Yield Strength 1120 MPa162000 psi
Notched Tensile Strength 1550 MPa225000 psiKt (stress concentration factor) = 6.1
Poissons Ratio 0.310.31After ST 720ºC , Aged 495ºC
Fatigue Strength  150 MPa
@# of Cycles 1.00e+7
21800 psi
@# of Cycles 1.00e+7
Kt (stress concentration factor) = 6.1 (STA sheet)
 290 MPa
@# of Cycles 30000
42100 psi
@# of Cycles 30000
Kt (stress concentration factor) = 6.1 (STA sheet)
 880 MPa
@# of Cycles 1.00e+7
128000 psi
@# of Cycles 1.00e+7
(plate), Unnotched
 925 MPa
@# of Cycles 100000
134000 psi
@# of Cycles 100000
unnotched
Shear Modulus 41.0 GPa5950 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000156 ohm-cm0.000156 ohm-cm
Magnetic Permeability 1.01.0
 
Thermal PropertiesMetricEnglishComments
CTE, linear  7.60 µm/m-°C
@Temperature 20.0 - 100 °C
4.22 µin/in-°F
@Temperature 68.0 - 212 °F
 8.10 µm/m-°C
@Temperature 20.0 - 315 °C
4.50 µin/in-°F
@Temperature 68.0 - 599 °F
average
 8.70 µm/m-°C
@Temperature 20.0 - 540 °C
4.83 µin/in-°F
@Temperature 68.0 - 1000 °F
average
Specific Heat Capacity 0.525 J/g-°C0.125 BTU/lb-°FTypical value for titanium alloys.
Thermal Conductivity 6.28 W/m-K43.6 BTU-in/hr-ft²-°F
Melting Point 1573 - 1690 °C2863 - 3070 °F
Solidus 1573 °C2863 °F
Liquidus 1690 °C3070 °F
Beta Transus 760 °C1400 °FSlow transition kinetics
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.10 %<= 0.10 %
Hydrogen, H <= 0.020 %<= 0.020 %
Iron, Fe <= 0.35 %<= 0.35 %
Molybdenum, Mo 11.5 %11.5 %
Nitrogen, N <= 0.050 %<= 0.050 %
Other, each <= 0.010 %<= 0.010 %
Other, total <= 0.040 %<= 0.040 %
Oxygen, O <= 0.18 %<= 0.18 %
Tin, Sn 4.5 %4.5 %
Titanium, Ti 78 %78 %
Zirconium, Zr 6.0 %6.0 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Titanium Beta III (Ti-11.5Mo-6Zr-4.5Sn; Grade 10), ST 720°C, Aged 550°C
Titanium Ti-11.5Mo-6Zr-4.5Sn, ST 720°C, Aged 495°C
Titanium Beta III (Ti-11.5Mo-6Zr-4.5Sn; Grade 10), ST 775°C, Aged 495°C
Titanium Beta III (Ti-11.5Mo-6Zr-4.5Sn; Grade 10), Solution Treated, Unaged
Titanium Beta III (Ti-11.5Mo-6Zr-4.5Sn; Grade 10), ST 720°C, Aged 580°C

MTB035 / 14157

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.