System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
Asahi Kasei Leona™ FR370 Polyamide 66, Flame Retardant
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 66 (PA66)
;
Nylon 66, Unreinforced, Flame Retardant
Material Notes:
Applications: Automotive parts, electrical & electronic parts, parts for office furnishings.
Information provided by Asahi Kasei Corp.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.16
g/cc
1.16
g/cc
Dry as Molded; ASTM D792
Density
1.16
g/cc
0.0419
lb/in³
Dry as Molded; ISO 1183
Moisture Absorption at Equilibrium
2.3 %
@Temperature 23.0 °C
2.3 %
@Temperature 73.4 °F
50% RH; ISO 62
2.3 %
@Temperature 23.0 °C
2.3 %
@Temperature 73.4 °F
50% RH
Linear Mold Shrinkage, Flow
0.0090
-
0.016
cm/cm
0.0090
-
0.016
in/in
Asahi Kasei
Mechanical Properties
Metric
English
Comments
Hardness, Rockwell M
55
55
Conditioned at 50% RH; ISO 2039
85
85
Dry as Molded; ISO 2039
Hardness, Rockwell R
110
110
Conditioned at 50% RH; ISO 2039
120
120
Dry as Molded; ISO 2039
Tensile Strength at Break
80.0
MPa
11600
psi
Conditioned at 50% RH; ISO 527
Tensile Strength
58.0
MPa
8410
psi
Conditioned at 50% RH; ASTM D638
83.0
MPa
12000
psi
Dry as Molded; ASTM D638
Tensile Strength, Yield
55.0
MPa
7980
psi
Conditioned at 50% RH
83.0
MPa
12000
psi
Dry as Molded
Elongation at Break
15 %
15 %
Dry as Molded; ISO 527
>= 50 %
>= 50 %
Conditioned at 50% RH; ISO 527
Elongation at Yield
4.5 %
@Temperature 23.0 °C
4.5 %
@Temperature 73.4 °F
Dry as Molded; ISO 527
22 %
@Temperature 23.0 °C
22 %
@Temperature 73.4 °F
Conditioned at 50% RH; ISO 527
Tensile Modulus
1.60
GPa
232
ksi
Conditioned at 50% RH; ISO 527
3.60
GPa
522
ksi
Dry as Molded; ISO 527
Flexural Strength
54.1
MPa
7850
psi
Conditioned at 50% RH; ISO 178
124
MPa
18000
psi
Dry as Molded; ISO 178
Flexural Modulus
1.50
GPa
218
ksi
Conditioned at 50% RH; ISO 178
2.60
GPa
377
ksi
Dry as Molded; ISO 178
Izod Impact, Notched
0.290
J/cm
0.543
ft-lb/in
Dry as Molded; ASTM D256
0.980
J/cm
1.84
ft-lb/in
Conditioned at 50% RH; ASTM D256
Charpy Impact Unnotched
5.80
J/cm²
27.6
ft-lb/in²
Dry as Molded; ISO 179
NB
NB
Conditioned at 50% RH; ISO 179
Charpy Impact, Notched
0.400
J/cm²
1.90
ft-lb/in²
Dry as Molded; ISO 179
0.600
J/cm²
2.86
ft-lb/in²
Conditioned at 50% RH; ISO 179
Electrical Properties
Metric
English
Comments
Volume Resistivity
1.00e+14
ohm-cm
1.00e+14
ohm-cm
Dry as Molded; IEC 60093
Surface Resistance
1.00e+13
ohm
1.00e+13
ohm
Dry as Molded; IEC 60093
Dielectric Strength
22.0
kV/mm
559
kV/in
Dry as Molded; IEC 60243
Comparative Tracking Index
600
V
@Thickness 3.00 mm
600
V
@Thickness 0.118 in
Dry as Molded; IEC 60112
Thermal Properties
Metric
English
Comments
CTE, linear
70.0
µm/m-°C
38.9
µin/in-°F
Dry as Molded; ASTMD 696
Deflection Temperature at 0.46 MPa (66 psi)
239
°C
462
°F
Dry as Molded; ISO 75
Deflection Temperature at 1.8 MPa (264 psi)
78.0
°C
172
°F
Dry as Molded; ISO 75
Flammability, UL94
V-0
@Thickness 0.750 mm
V-0
@Thickness 0.0295 in
Dry as Molded
Oxygen Index
36 %
36 %
Dry as Molded; ASTM D2863
Glow Wire Flammability Index
960
°C
1760
°F
Dry as Molded; IEC 60695-2-12
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
RTP Company RTP 200 TFE 20 FR Nylon 6/6 (PA), PTFE Lubricated - Flame Retardant
Celanese Zytel® FR7025V0F NC010 PA66-FR(30)
PASAHI8162 / 221189
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.