MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

ATI Allegheny Ludlum AL 453™ Stainless Steel
Categories: Metal; Ferrous Metal; Ferritic; Stainless Steel

Material Notes: Single phase iron-chromium ferritic stainless steel alloy. Should be annealed between 1450 and 1600°F and quickly cooled.

Information provided by Allegheny Ludlum

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.61 g/cc0.275 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 7878
Tensile Strength, Ultimate 470 MPa68200 psi
 20.0 MPa
@Temperature 1093 °C
2900 psi
@Temperature 1999 °F
 33.0 MPa
@Temperature 871 °C
4790 psi
@Temperature 1600 °F
 60.0 MPa
@Temperature 760 °C
8700 psi
@Temperature 1400 °F
 120 MPa
@Temperature 649 °C
17400 psi
@Temperature 1200 °F
 251 MPa
@Temperature 538 °C
36400 psi
@Temperature 1000 °F
 345 MPa
@Temperature 427 °C
50000 psi
@Temperature 801 °F
 409 MPa
@Temperature 204 °C
59300 psi
@Temperature 399 °F
Tensile Strength, Yield  23.0 MPa
@Temperature 871 °C
3340 psi
@Temperature 1600 °F
 39.0 MPa
@Temperature 760 °C
5660 psi
@Temperature 1400 °F
 82.0 MPa
@Temperature 649 °C
11900 psi
@Temperature 1200 °F
 173 MPa
@Temperature 538 °C
25100 psi
@Temperature 1000 °F
 183 MPa
@Temperature 427 °C
26500 psi
@Temperature 801 °F
 218 MPa
@Temperature 204 °C
31600 psi
@Temperature 399 °F
 310 MPa
@Strain 0.2 %
45000 psi
@Strain 0.2 %
Elongation at Break 35 %35 %in 2"
 21.5 %
@Temperature 427 °C
21.5 %
@Temperature 801 °F
 25.8 %
@Temperature 538 °C
25.8 %
@Temperature 1000 °F
 26.8 %
@Temperature 204 °C
26.8 %
@Temperature 399 °F
 76.6 %
@Temperature 649 °C
76.6 %
@Temperature 1200 °F
 95 %
@Temperature 760 °C
95 %
@Temperature 1400 °F
 95.5 %
@Temperature 982 °C
95.5 %
@Temperature 1800 °F
 98.1 %
@Temperature 871 °C
98.1 %
@Temperature 1600 °F
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000733 ohm-cm0.0000733 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  10.2 µm/m-°C
@Temperature 20.0 - 100 °C
5.67 µin/in-°F
@Temperature 68.0 - 212 °F
 11.4 µm/m-°C
@Temperature 20.0 - 538 °C
6.33 µin/in-°F
@Temperature 68.0 - 1000 °F
 14.0 µm/m-°C
@Temperature 20.0 - 1093 °C
7.78 µin/in-°F
@Temperature 68.0 - 1999 °F
Thermal Conductivity 19.2 W/m-K133 BTU-in/hr-ft²-°F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 0.60 %0.60 %
Carbon, C 0.030 %0.030 %
Chromium, Cr 22 %22 %
Iron, Fe >= 76.3 %>= 76.3 %As Remainder
Manganese, Mn 0.30 %0.30 %
Nickel, Ni 0.30 %0.30 %
Phosphorus, P 0.020 %0.020 %
Rare Earths <= 0.10 %<= 0.10 %
Silicon, Si 0.30 %0.30 %
Sulfur, S <= 0.030 %<= 0.030 %
Titanium, Ti 0.020 %0.020 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ASTM A500 Steel, grade A, Round Structural Tubing
Morgan Advanced Ceramics Kao-Lok® Hardware for Blanket Wallpaper Systems 304SS Washers and Studs
Cotronics Resbond™ 954 High Temperature Ceramic Adhesive, Stainless Steel Composition
ATI Allegheny Ludlum AL 4565™ Corrosion Resistant Stainless Steel
ASTM A501 Steel

NL1021 / 17789

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.