MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Akro-Plastic Akromid® T1 GF 50 9 (3257) PPA Dry, 50% Glass Filled
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA); Polyphthalamide (PPA), 50% Glass Fiber Reinforced

Material Notes: AKROMID® T is characterized primarily by high heat resistance and the lowest moisture absorption of the manufacturer's PA grades, making it particularly suited in the automotive sector for high-temperature applications in the engine compartment and in machine building for components subjected to high mechanical loads. It easily maintains its high initial stability even at temperatures of up to 140 °C and still exhibits excellent creep behavior. This high dimensional stability is further enhanced by the product’s low moisture absorption. Another advantage over PA 6 or PA 6.6 is the improved chemical resistance and high resistance to hydrolytic degradation. These properties – along with the aforementioned advantages in terms of mechanical loading – make the material useful for difficult applications in industrial pumps and fluid filters. Its low water absorption over extended periods is yet another advantage. By modifying the base grades, the material can be suitable for applications requiring a high quality surface finish.

Applications:

    Automotive Sector:
  • Cooling system (thermostat housing, connectors, etc.)
  • Parts in the oil circuit (tensioner bases, etc.)
  • Parts in the brake system (valve bodies, etc.)
  • Clutch components (central clutch release bearing, etc.)
  • Air ducting parts (side pieces for charge-air coolers, control shafts, etc.)
  • Parts subjected to high loads in the interior (centre armrest, etc.)
    Electrical Engineering:
  • Mobile telephone parts (chip carrier, etc.)
  • Coil formers
  • Motor parts (brush holders, etc.)
  • Plugs and connectors
  • Bulb and LED sockets
    Industry and Household:
  • Heating systems (fan housings, etc.)
  • Components for coffee machines (grades compliant with KTW- German recommendation for polymers in drinking-water systems)
  • Water counters and water filters (KTW-compliant, hot water)
  • Pump systems (misc. functional parts)

Information from Akro-Plastic

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.62 g/cc
@Temperature 23.0 °C
0.0585 lb/in³
@Temperature 73.4 °F
ISO 1183
Filler Content 50 %50 %ISO 1172
Moisture Absorption 0.95 %
@Temperature 70.0 °C
0.95 %
@Temperature 158 °F
62% r.h.; ISO 62
Linear Mold Shrinkage, Flow 0.0020 cm/cm0.0020 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.0070 cm/cm0.0070 in/inISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 340 MPa49300 psiISO 2039-1
Tensile Strength at Break 290 MPa42100 psi5 [mm/min]; ISO 527-1/2
 145 MPa
@Treatment Temp. 150 - 160 °C,
Time 1.80e+7 sec
21000 psi
@Treatment Temp. 302 - 320 °F,
Time 5000 hour
5 [mm/min], 50% Loss of Tensile Strength; ICE 216
 145 MPa
@Treatment Temp. 130 - 140 °C,
Time 7.20e+7 sec
21000 psi
@Treatment Temp. 266 - 284 °F,
Time 20000 hour
5 [mm/min], 50% Loss of Tensile Strength; ICE 216
Elongation at Break 2.1 %2.1 %5 [mm/min]; ISO 527-1/2
Tensile Modulus 19.5 GPa2830 ksi1[mm/min]; ISO 527-1/2
Flexural Strength 390 MPa56600 psi2 [mm/min]; ISO 178
Flexural Modulus 17.0 GPa2470 ksi2 [mm/min]; ISO 178
Flexural Strain at Break 2.6 %2.6 %2 mm/min; ISO 178
Shear Modulus  0.350 GPa
@Temperature 350 °C
50.8 ksi
@Temperature 662 °F
 0.400 GPa
@Temperature 300 °C
58.0 ksi
@Temperature 572 °F
 0.500 GPa
@Temperature 250 °C
72.5 ksi
@Temperature 482 °F
 0.600 GPa
@Temperature 200 °C
87.0 ksi
@Temperature 392 °F
 2.00 GPa
@Temperature 150 °C
290 ksi
@Temperature 302 °F
 3.00 GPa
@Temperature 100 °C
435 ksi
@Temperature 212 °F
 4.00 GPa
@Temperature 0.000 °C
580 ksi
@Temperature 32.0 °F
Charpy Impact Unnotched  8.00 J/cm²
@Temperature -30.0 °C
38.1 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
 9.00 J/cm²
@Temperature 23.0 °C
42.8 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched  1.40 J/cm²
@Temperature 23.0 °C
6.66 ft-lb/in²
@Temperature 73.4 °F
ISO 179-1/1eA
 1.40 J/cm²
@Temperature -30.0 °C
6.66 ft-lb/in²
@Temperature -22.0 °F
ISO 179-1/1eA
 
Electrical PropertiesMetricEnglishComments
Comparative Tracking Index 600 V600 VTest Solution A; IEC 60112
 
Thermal PropertiesMetricEnglishComments
Melting Point 308 °C586 °FISO 11357-1, DSC,10 [K/min]
Deflection Temperature at 1.8 MPa (264 psi) 275 °C527 °FHDT/A; ISO 75-1/2
Deflection Temperature at 8.0 MPa 205 °C401 °FHDT/C; ISO 75-1/2
Flammability, UL94 HB
@Thickness 0.800 mm
HB
@Thickness 0.0315 in
Glow Wire Ignition Temperature 725 °C
@Thickness 1.60 mm
1340 °F
@Thickness 0.0630 in
IEC 60695-2-13
Glow Wire Flammability Index 700 °C
@Thickness 1.60 mm
1290 °F
@Thickness 0.0630 in
IEC 60695-2-12
 
Processing PropertiesMetricEnglishComments
Feed Temperature 80.0 - 95.0 °C176 - 203 °F
Nozzle Temperature 320 - 330 °C608 - 626 °F
Zone 1 310 - 320 °C590 - 608 °F
Zone 2 315 - 325 °C599 - 617 °F
Zone 3 320 - 335 °C608 - 635 °F
Zone 4 320 - 335 °C608 - 635 °F
Melt Temperature 325 - 340 °C617 - 644 °F
Mold Temperature 100 - 130 °C212 - 266 °F
Drying Temperature 90.0 °C194 °F
Dry Time 2 - 16.0 hour2 - 16.0 hour
Moisture Content <= 0.10 %<= 0.10 %
Hold Pressure 30.0 - 80.0 MPa4350 - 11600 psi
Back Pressure 0.200 - 0.650 MPa29.0 - 94.3 psi
 
Descriptive Properties
Acetic acidFail100% Conc
AcetonePass100% Conc
CresolFail100% Conc
Diesel fuel (DIN 51601)Pass100% Conc
Engine oilPass100% Conc
EthanolPass96% Conc
Ethylene glycol/waterPass120°C, 50% Conc
Formic acidFail100% Conc
Hydraulic oilPass100% Conc
Injection Speedaverage to high
IsopropanolPass100% Conc
KerosenePass100% Conc
MethanolPass100% Conc
PetrolPass100% Conc
PhenolFail100% Conc
Rate acc. FMVSS 302 (<100/min)Passed
Rate acc. FMVSS 302,(<100/min)FMVSS 302, >1 [mm] Thickness
Silicone oilPass
Sulfuric AcidFail96% Conc
ToluenePass100% Conc
Urea, aqueousPass20% Conc
WaterPass100% Conc
XylenePass100% Conc
Zinc chloride, aqueousPass50% Conc

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polyphthalamide (PPA), 30% Glass Fiber Reinforced
Overview of materials for Polyphthalamide (PPA), 50% Glass Fiber Reinforced
Akro-Plastic Akromid® T1 GF 50 9 (3257) PPA Conditioned, 50% Glass Filled
Celanese Zytel® HTN 51G50HSL BK083 Polyphthalamide (PPA) (Extended Tabular Stress-Strain Data)
Overview of materials for Polyphthalamide (PPA)

PAKRO063 / 126843

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.