MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Outokumpu 4762 High Temperature Ferritic Stainless Steel
Categories: Metal; Ferrous Metal; Ferritic; Stainless Steel

Material Notes: Highest chromium content-most resistant to reducing sulphurous gases. Susceptible to 475°C embrittlement and s-phase forms during long exposures in the range 600-800°C.

Applications: Mostly used in high temperature applications with sulphurous atmospheres and/or low tensile loads such as for installations within:

  • Chemical industry (drums)
  • Power industry (coal burners)
  • Metalworking industry (heat treatment boxes)
  • Furnace technology (walls, doors)

Available in hot rolled plate (Quarto) form.

Key Words: EN 1.4762; UNS S44600
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.50 g/cc0.271 lb/in³RT
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 223223RT; EN 10003-1
Tensile Strength, Ultimate 555 MPa80500 psiOutokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
Tensile Strength, Yield  405 MPa
@Strain 0.2 %
58700 psi
@Strain 0.2 %
Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
 440 MPa
@Strain 1 %
63800 psi
@Strain 1 %
Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
Elongation at Break 30 %30 %Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000102 ohm-cm0.000102 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  12.0 µm/m-°C
@Temperature 600 °C
6.67 µin/in-°F
@Temperature 1110 °F
 12.9 µm/m-°C
@Temperature 800 °C
7.17 µin/in-°F
@Temperature 1470 °F
 14.0 µm/m-°C
@Temperature 1000 °C
7.78 µin/in-°F
@Temperature 1830 °F
Specific Heat Capacity 0.460 J/g-°C0.110 BTU/lb-°FRT
Thermal Conductivity 14.2 W/m-K98.5 BTU-in/hr-ft²-°FRT
 20.9 W/m-K
@Temperature 500 °C
145 BTU-in/hr-ft²-°F
@Temperature 932 °F
Maximum Service Temperature, Air 1150 °C2100 °FDry Air
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 800 - 850 °C1470 - 1560 °FCooling: forced air or water
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 1.2 %1.2 %
Carbon, C 0.12 %0.12 %
Chromium, Cr 24 %24 %
Iron, Fe 74.68 %74.68 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Sandvik 4C54 Seamless tube and pipe
446 Stainless Steel, Annealed Sheet
446 Stainless Steel, Annealed Plate
446 Stainless Steel, Annealed Bar
446 Stainless Steel, Annealed and Cold Drawn Bar

NOUTOK39 / 18754

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.