MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Lubrizol Estane® 2103-90AEL Film Grade Thermoplastic Polyurethane Elastomer
Categories: Polymer; Film; Thermoplastic; Elastomer, TPE; Polyurethane, TP; Thermoplastic Polyurethane, Elastomer, Ether Grade

Material Notes: Formerly Pellethane

Feature: Film resin for injection blow molding

Available in Americas, Europe, Middle East, Africa, India and Asia

Data provided by Lubrizol.

Lubrizol acquired the Pellethane product line from Dow in 2009.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.14 g/cc1.14 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0050 - 0.0080 cm/cm0.0050 - 0.0080 in/inASTM D955
Linear Mold Shrinkage, Transverse 0.0040 - 0.0050 cm/cm0.0040 - 0.0050 in/inASTM D955
Melt Flow 6.0 g/10 min
@Load 8.70 kg,
Temperature 224 °C
6.0 g/10 min
@Load 19.2 lb,
Temperature 435 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 9292ASTM D2240
Tensile Strength, Ultimate 38.9 MPa5640 psiASTM D412
Elongation at Break 480 %480 %ASTM D412
50% Modulus 6.90 MPa
@Strain 50 %
6.90 MPa
@Strain 50 %
ASTM D412
100% Modulus 9.70 MPa
@Strain 100 %
1410 psi
@Strain 100 %
ASTM D412
300% Modulus 20.3 MPa
@Strain 300 %
2940 psi
@Strain 300 %
ASTM D412
Flexural Modulus 0.0689 GPa10.0 ksiASTM D790
Tear Strength 94.6 kN/m540 pliDie C; ASTM D624
Taber Abrasion, mg/1000 Cycles 5050H-22 wheel (coarser), 1000g; ASTM D1044
Compression Set 40 %
@Temperature 70.0 °C
40 %
@Temperature 158 °F
22 hrs.; ASTM D395, Method B
 25 %
@Temperature 25.0 °C,
Time 79200 sec
25 %
@Temperature 77.0 °F,
Time 22.0 hour
ASTM D395, Method B
Tensile Set 60 %60 %Elongation Set After Break; ASTM D412
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 156 µm/m-°C
@Temperature 20.0 °C
86.7 µin/in-°F
@Temperature 68.0 °F
ASTM D696
Vicat Softening Point 102 °C216 °F120°C/hr, 9.8N; ASTM D1525
Glass Transition Temp, Tg -27.0 °C-16.6 °FDSC
 
Processing PropertiesMetricEnglishComments
Melt Temperature 188 - 204 °C370 - 399 °FExtrusion
 193 - 210 °C379 - 410 °FMolding
Mold Temperature 16.0 - 60.0 °C60.8 - 140 °F
Drying Temperature 88.0 - 104 °C190 - 219 °Fair dew point <-40°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Huntsman IROGRAN® A 78 E 4723 Polyester-Based TPU-Injection Extrusion Grade
Covestro Desmopan® 2590A Thermoplastic Polyurethane
Huntsman IROGRAN® A 92 E 4694 Polyester-Based TPU-Injection Extrusion Grade
Huntsman IROGRAN® A 95 E 4813 Polyester-Based TPU-High Performance Grade
Huntsman IROGRAN® A 70 H 4673 M Polyester-Based TPU-Injection Molding Grade

PDW294a / 138269

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.