MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

AISI 1030 Steel, water quenched from 870°C (1600°F), 650°C (1200°F) temper, 25 mm (1 in.) round
Categories: Metal; Ferrous Metal; Carbon Steel; AISI 1000 Series Steel; Medium Carbon Steel

Material Notes: Applications include levers, bolts, studs, nuts, and similar parts which are headed, upset, or extruded. Wires uses include nails requiring high shank rigidity or strength and quench-hardened nails. Post water quenched hardness: 46 HRC surface, 23 HRC half-radius, 21 HRC surface

Key Words: UNS G10300, ASTM A29, ASTM A108, ASTM A510, ASTM A512, ASTM A519, ASTM A544, ASTM A545, ASTM A546, ASTM A576, ASTM A682, FED QQ-S-635 (C1030), FED QQ-S-700 (C1030), MIL SPEC MIL-S-11310 (CS1030), SAE J403, SAE J412, SAE J414, DIN 1.1172, UNI CB 35
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.87 g/cc0.284 lb/in³Typical for steels.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 170170
Hardness, Knoop 191191Converted from Brinell
Hardness, Rockwell B 8686Converted from Brinell
Hardness, Vickers 178178Converted from Brinell
Tensile Strength, Ultimate 580 MPa84100 psi
Tensile Strength, Yield 425 MPa61600 psi
Elongation at Break 28.5 %28.5 %in 50 mm
Reduction of Area 71.4 %71.4 %
Modulus of Elasticity 206 GPa29900 ksi
Bulk Modulus 163 GPa23600 ksiEstimated from elastic modulus
Poissons Ratio 0.290.29Typical for steel
Shear Modulus 80.0 GPa11600 ksiEstimated from elastic modulus
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000166 ohm-cm
@Temperature 20.0 °C
0.0000166 ohm-cm
@Temperature 68.0 °F
annealed specimen
 
Thermal PropertiesMetricEnglishComments
CTE, linear 11.7 µm/m-°C
@Temperature 15.0 - 75.0 °C
6.50 µin/in-°F
@Temperature 59.0 - 167 °F
Specific Heat Capacity 0.486 J/g-°C
@Temperature >=100 °C
0.116 BTU/lb-°F
@Temperature >=212 °F
annealed
Thermal Conductivity  43.6 W/m-K
@Temperature 100 °C
303 BTU-in/hr-ft²-°F
@Temperature 212 °F
Estimated
 50.7 W/m-K
@Temperature 0.000 °C
352 BTU-in/hr-ft²-°F
@Temperature 32.0 °F
Estimated
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.27 - 0.34 %0.27 - 0.34 %
Iron, Fe 98.67 - 99.13 %98.67 - 99.13 %As remainder
Manganese, Mn 0.60 - 0.90 %0.60 - 0.90 %
Phosphorus, P <= 0.040 %<= 0.040 %
Sulfur, S <= 0.050 %<= 0.050 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI 1030 Steel, water quenched from 870°C (1600°F), 540°C (1000°F) temper, 25 mm (1 in.) round
AISI 1030 Steel, water quenched from 870°C (1600°F), 540°C (1000°F) temper, 50 mm (2 in.) round
AISI 1030 Steel, water quenched from 870°C (1600°F), 540°C (1000°F) temper, 13 mm (0.5 in.) round
AISI 1030 Steel, water quenched from 870°C (1600°F), 540°C (1000°F) temper, 100 mm (4 in.) round
AISI 1030 Steel, water quenched from 870°C (1600°F), 650°C (1200°F) temper, 13 mm (0.5 in.) round

M1030T / 6908

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.