MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Polypropylene with 20% Talc Filler
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene with 20% Talc Filler

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polypropylene with 20% Talc Filler".Specific grades with primary filler content between 15% and 24% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 0.980 - 1.46 g/cc0.0354 - 0.0527 lb/in³Average value: 1.04 g/cc Grade Count:904
Filler Content 15.0 - 23.0 %15.0 - 23.0 %Average value: 19.4 % Grade Count:192
Water Absorption 0.000 - 0.0500 %0.000 - 0.0500 %Average value: 0.0327 % Grade Count:26
Moisture Absorption at Equilibrium 0.0100 - 0.100 %0.0100 - 0.100 %Average value: 0.0467 % Grade Count:3
Maximum Moisture Content  0.200 - 0.200
@Temperature 120 - 120 °C
0.200 - 0.200
@Temperature 248 - 248 °F
Average value: 0.200 Grade Count:4
 0.200 - 0.200
@Time 299 - 299 sec
0.200 - 0.200
@Time 0.0830 - 0.0830 hour
Average value: 0.200 Grade Count:4
Linear Mold Shrinkage 0.000900 - 0.0265 cm/cm0.000900 - 0.0265 in/inAverage value: 0.0119 cm/cm Grade Count:302
 0.00800 - 0.00800 cm/cm
@Temperature 80.0 - 80.0 °C
0.00800 - 0.00800 in/in
@Temperature 176 - 176 °F
Average value: 0.00800 cm/cm Grade Count:1
Linear Mold Shrinkage, Transverse 0.00500 - 0.0272 cm/cm0.00500 - 0.0272 in/inAverage value: 0.0124 cm/cm Grade Count:112
 0.0100 - 0.0100 cm/cm
@Temperature 80.0 - 80.0 °C
0.0100 - 0.0100 in/in
@Temperature 176 - 176 °F
Average value: 0.0100 cm/cm Grade Count:1
Melt Flow 0.500 - 90.0 g/10 min0.500 - 90.0 g/10 minAverage value: 15.6 g/10 min Grade Count:874
Ash 15.0 - 30.0 %15.0 - 30.0 %Average value: 20.1 % Grade Count:37
 15.0 - 24.0 %
@Temperature 600 - 700 °C
15.0 - 24.0 %
@Temperature 1110 - 1290 °F
Average value: 19.8 % Grade Count:12
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 48.0 - 10048.0 - 100Average value: 67.8 Grade Count:4
Hardness, Rockwell R 52.0 - 10752.0 - 107Average value: 86.4 Grade Count:49
Hardness, Shore D 56.0 - 80.056.0 - 80.0Average value: 69.7 Grade Count:70
Ball Indentation Hardness 39.0 - 60.0 MPa5660 - 8700 psiAverage value: 52.2 MPa Grade Count:6
Tensile Strength, Ultimate 6.00 - 37.0 MPa870 - 5370 psiAverage value: 26.1 MPa Grade Count:290
Tensile Strength, Yield 12.0 - 37.0 MPa1740 - 5370 psiAverage value: 23.4 MPa Grade Count:533
Elongation at Break 3.00 - 550 %3.00 - 550 %Average value: 47.6 % Grade Count:261
Elongation at Yield 3.00 - 32.0 %3.00 - 32.0 %Average value: 8.19 % Grade Count:149
Modulus of Elasticity 1.10 - 3.45 GPa160 - 500 ksiAverage value: 2.21 GPa Grade Count:138
Flexural Yield Strength 17.0 - 70.0 MPa2470 - 10200 psiAverage value: 42.1 MPa Grade Count:224
Flexural Modulus 0.800 - 3.59 GPa116 - 520 ksiAverage value: 2.02 GPa Grade Count:889
 0.470 - 2.40 GPa
@Temperature -20.0 - 100 °C
68.2 - 348 ksi
@Temperature -4.00 - 212 °F
Average value: 1.81 GPa Grade Count:6
Izod Impact, Notched 0.198 - 981 J/cm0.370 - 1840 ft-lb/inAverage value: 0.702 J/cm Grade Count:207
 0.140 - 0.26695 J/cm
@Temperature -40.0 - -20.0 °C
0.262 - 0.50011 ft-lb/in
@Temperature -40.0 - -4.00 °F
Average value: 0.201 J/cm Grade Count:5
Izod Impact, Unnotched 0.200 - 5340 J/cm0.375 - 10000 ft-lb/inAverage value: 5.36 J/cm Grade Count:48
 0.250 - 0.250 J/cm
@Temperature 0.000 - 0.000 °C
0.468 - 0.468 ft-lb/in
@Temperature 32.0 - 32.0 °F
Average value: 0.250 J/cm Grade Count:2
Izod Impact, Notched (ISO) 2.40 - 181 kJ/m²1.14 - 85.9 ft-lb/in²Average value: 25.5 kJ/m² Grade Count:265
 1.70 - 25.0 kJ/m²
@Temperature -40.0 - 0.000 °C
0.809 - 11.9 ft-lb/in²
@Temperature -40.0 - 32.0 °F
Average value: 4.73 kJ/m² Grade Count:157
Izod Impact, Unnotched (ISO) 15.0 - 55.0 kJ/m²7.14 - 26.2 ft-lb/in²Average value: 32.0 kJ/m² Grade Count:9
 17.0 - 24.0 kJ/m²
@Temperature -30.0 - -30.0 °C
8.09 - 11.4 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 20.5 kJ/m² Grade Count:2
Charpy Impact Unnotched 1.30 J/cm² - NB6.19 ft-lb/in² - NBAverage value: 4.71 J/cm² Grade Count:198
 0.450 J/cm² - NB
@Temperature -40.0 - 0.000 °C
2.14 ft-lb/in² - NB
@Temperature -40.0 - 32.0 °F
Average value: 2.44 J/cm² Grade Count:76
Charpy Impact, Notched 0.160 - 7.50 J/cm²0.761 - 35.7 ft-lb/in²Average value: 2.01 J/cm² Grade Count:476
 0.100 - 4.80 J/cm²
@Temperature -40.0 - 0.000 °C
0.476 - 22.8 ft-lb/in²
@Temperature -40.0 - 32.0 °F
Average value: 0.365 J/cm² Grade Count:323
Gardner Impact 0.451 - 271 J0.333 - 200 ft-lbAverage value: 13.4 J Grade Count:75
 1.35582 - 43.3862 J
@Temperature -30.0 - -5.56 °C
1.00000 - 32.0000 ft-lb
@Temperature -22.0 - 22.0 °F
Average value: 13.7 J Grade Count:4
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 2.00e+15 - 1.00e+16 ohm-cm2.00e+15 - 1.00e+16 ohm-cmAverage value: 8.00e+15 ohm-cm Grade Count:12
Surface Resistance 1.00e+13 ohm1.00e+13 ohmAverage value: 1.00e+13 ohm Grade Count:6
Dielectric Constant 2.35 - 2.502.35 - 2.50Average value: 2.38 Grade Count:6
Dielectric Strength 19.7 - 24.0 kV/mm500 - 610 kV/inAverage value: 21.1 kV/mm Grade Count:3
Comparative Tracking Index 600 V600 VAverage value: 600 V Grade Count:15
 
Thermal PropertiesMetricEnglishComments
CTE, linear 50.0 - 110 µm/m-°C27.8 - 61.1 µin/in-°FAverage value: 70.3 µm/m-°C Grade Count:35
Melting Point 135 - 193 °C275 - 379 °FAverage value: 161 °C Grade Count:35
Maximum Service Temperature, Air 65.0 - 135 °C149 - 275 °FAverage value: 103 °C Grade Count:4
Hot Ball Pressure Test 125 °C257 °FAverage value: 125 °C Grade Count:6
Deflection Temperature at 0.46 MPa (66 psi) 55.0 - 145 °C131 - 293 °FAverage value: 108 °C Grade Count:568
Deflection Temperature at 1.8 MPa (264 psi) 35.0 - 174 °C95.0 - 345 °FAverage value: 66.0 °C Grade Count:461
Vicat Softening Point 45.0 - 160 °C113 - 320 °FAverage value: 112 °C Grade Count:297
Flammability, UL94 HB - 5VAHB - 5VAGrade Count:164
Flame Spread 15.2 - 22.9 mm/min0.600 - 0.900 in/minAverage value: 19.8 mm/min Grade Count:5
Oxygen Index 21.0 %21.0 %Average value: 21.0 % Grade Count:8
Glow Wire Test 550 - 960 °C1020 - 1760 °FAverage value: 733 °C Grade Count:63
 
Optical PropertiesMetricEnglishComments
Gloss 45.0 - 47.0 %45.0 - 47.0 %Average value: 46.0 % Grade Count:4
 
Processing PropertiesMetricEnglishComments
Processing Temperature 193 - 227 °C380 - 440 °FAverage value: 210 °C Grade Count:8
Nozzle Temperature 193 - 260 °C380 - 500 °FAverage value: 219 °C Grade Count:79
Adapter Temperature 200 - 210 °C392 - 410 °FAverage value: 205 °C Grade Count:4
Die Temperature 190 - 220 °C374 - 428 °FAverage value: 205 °C Grade Count:6
Melt Temperature 160 - 280 °C320 - 536 °FAverage value: 219 °C Grade Count:241
Mold Temperature 10.0 - 90.0 °C50.0 - 194 °FAverage value: 47.6 °C Grade Count:242
Drying Temperature 51.7 - 220 °C125 - 428 °FAverage value: 78.6 °C Grade Count:193
Moisture Content 0.0500 - 0.100 %0.0500 - 0.100 %Average value: 0.0524 % Grade Count:62
Injection Pressure 2.76 - 140 MPa400 - 20300 psiAverage value: 59.7 MPa Grade Count:170

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polypropylene, Molded
Overview of materials for Polypropylene with 20% Glass Fiber Filler
Overview of materials for Polypropylene with 10% Talc Filler
Overview of materials for Polypropylene with 40% Talc Filler
Overview of materials for Polypropylene with 30% Talc Filler

O4762 / 78399

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.