MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Bohler-Uddeholm BÖHLER M303 EXTRA Plastic Mold Steel
Categories: Metal; Ferrous Metal; Tool Steel; Mold Steel

Material Notes: BOHLER M303 EXTRA is a stainless martensitic chromium steel, offering excellent toughness, corrosion and wear resistance. It is characterized by improved machinability and polishability. BOHLER M303 EXTRA was developed for improved homogeneity over DIN 1.2316 by reducing delta ferrite in the matrix, ensuring excellent usage properties.

Applications

  • Molds for chemically aggressive plastics
  • Molds for household appliances
  • Vinyl Extrusion tools
  • Molds for fittings

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.70 g/cc0.278 lb/in³
 7.60 g/cc
@Temperature 400 °C
0.275 lb/in³
@Temperature 752 °F
 7.60 g/cc
@Temperature 500 °C
0.275 lb/in³
@Temperature 932 °F
 7.60 g/cc
@Temperature 600 °C
0.275 lb/in³
@Temperature 1110 °F
 7.70 g/cc
@Temperature 100 °C
0.278 lb/in³
@Temperature 212 °F
 7.70 g/cc
@Temperature 200 °C
0.278 lb/in³
@Temperature 392 °F
 7.70 g/cc
@Temperature 300 °C
0.278 lb/in³
@Temperature 572 °F
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 290 - 330290 - 330as supplied; hardened and tempered
Hardness, Rockwell C 5353hardening at 1020°C; without tempering
Modulus of Elasticity  168 GPa
@Temperature 600 °C
24400 ksi
@Temperature 1110 °F
 181 GPa
@Temperature 500 °C
26300 ksi
@Temperature 932 °F
 191 GPa
@Temperature 400 °C
27700 ksi
@Temperature 752 °F
 200 GPa
@Temperature 300 °C
29000 ksi
@Temperature 572 °F
 207 GPa
@Temperature 200 °C
30000 ksi
@Temperature 392 °F
 214 GPa
@Temperature 100 °C
31000 ksi
@Temperature 212 °F
 218 GPa
@Temperature 20.0 °C
31600 ksi
@Temperature 68.0 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  10.5 µm/m-°C
@Temperature 20.0 - 100 °C
5.83 µin/in-°F
@Temperature 68.0 - 212 °F
 10.8 µm/m-°C
@Temperature 20.0 - 200 °C
6.00 µin/in-°F
@Temperature 68.0 - 392 °F
 11.1 µm/m-°C
@Temperature 20.0 - 300 °C
6.17 µin/in-°F
@Temperature 68.0 - 572 °F
 11.4 µm/m-°C
@Temperature 20.0 - 400 °C
6.33 µin/in-°F
@Temperature 68.0 - 752 °F
 11.7 µm/m-°C
@Temperature 20.0 - 500 °C
6.50 µin/in-°F
@Temperature 68.0 - 932 °F
 12.1 µm/m-°C
@Temperature 20.0 - 600 °C
6.72 µin/in-°F
@Temperature 68.0 - 1110 °F
Specific Heat Capacity  0.460 J/g-°C
@Temperature 20.0 °C
0.110 BTU/lb-°F
@Temperature 68.0 °F
 0.484 J/g-°C
@Temperature 100 °C
0.116 BTU/lb-°F
@Temperature 212 °F
 0.529 J/g-°C
@Temperature 200 °C
0.126 BTU/lb-°F
@Temperature 392 °F
 0.564 J/g-°C
@Temperature 300 °C
0.135 BTU/lb-°F
@Temperature 572 °F
 0.615 J/g-°C
@Temperature 400 °C
0.147 BTU/lb-°F
@Temperature 752 °F
 0.694 J/g-°C
@Temperature 500 °C
0.166 BTU/lb-°F
@Temperature 932 °F
 0.795 J/g-°C
@Temperature 600 °C
0.190 BTU/lb-°F
@Temperature 1110 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.27 %0.27 %
Chromium, Cr 14.5 %14.5 %
Iron, Fe 82.4 %82.4 %As Balance
Manganese, Mn 0.65 %0.65 %
Molybdenum, Mo 1.0 %1.0 %
Nickel, Ni 0.85 %0.85 %
Silicon, Si 0.30 %0.30 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Bohler-Uddeholm UDDEHOLM RAMAX® LH Plastic Mold Steel
AISI Type H13 Hot Work Tool Steel
Bohler-Uddeholm UDDEHOLM ELMAX® Powder Metallurgy Stainless Mold Steel
Bohler-Uddeholm UDDEHOLM CORRAX® Precipitation Hardening Stainless Mold Steel
420 Stainless Steel

NBUCOR43 / 98122

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.