MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Covestro Texin® 245 Thermoplastic Polyurethanes (TPU) (Extended Aging Data)
Categories: Polymer; Thermoplastic; Polyurethane, TP

Material Notes: Texin 245 resin is an aromatic polyester-based thermoplastic polyurethane with a Shore hardness of approximately 43D. It can be processed by injection molding; extrusion processes are not recommended.

Properties / Applications: Texin 245 resin is characterized by excellent low-temperature properties and excellent fuel and oil resistance. It also offers outstanding abrasion resistance, impact strength, toughness, and flexibility. Texin 245 natural color resin complies with FDA food-contact regulations 21 CFR 177.1680 (Polyurethane Resins) and 177.2600 (Rubber Articles Intended for Repeated Use), subject to the limitations of these and any other applicable regulations. Typical applications include casters, couplings, sleeves and gears.

Information provided by Covestro

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.21 g/cc1.21 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0080 cm/cm
@Thickness 2.54 mm
0.0080 in/in
@Thickness 0.100 in
ASTM D955
Linear Mold Shrinkage, Transverse 0.0080 cm/cm
@Thickness 2.54 mm
0.0080 in/in
@Thickness 0.100 in
ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 4343ASTM D2240
 32
@Time 252000 sec
32
@Time 70.0 hour
Fuel C; ASTM D471
 32
@Time 605000 sec
32
@Time 168 hour
Fuel C; ASTM D471
 32
@Time 1.21e+6 sec
32
@Time 336 hour
Fuel C; ASTM D471
 32
@Time 1.81e+6 sec
32
@Time 504 hour
Fuel C; ASTM D471
 41
@Time 252000 sec
41
@Time 70.0 hour
Fuel A; ASTM D471
 41
@Time 605000 sec
41
@Time 168 hour
Fuel A; ASTM D471
 42
@Time 1.81e+6 sec
42
@Time 504 hour
Fuel A; ASTM D471
 43
@Time 1.21e+6 sec
43
@Time 336 hour
Fuel A; ASTM D471
 38
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
38
@Treatment Temp. 212 °F,
Time 504 hour
ASTM Oil #1; ASTM D471
 38
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
38
@Treatment Temp. 212 °F,
Time 336 hour
ASTM Oil #1; ASTM D471
 38
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
38
@Treatment Temp. 212 °F,
Time 504 hour
Hot Air; ASTM D573
 39
@Treatment Temp. 100 °C,
Time 605000 sec
39
@Treatment Temp. 212 °F,
Time 168 hour
Hot Air; ASTM D573
 39
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
39
@Treatment Temp. 212 °F,
Time 336 hour
Hot Air; ASTM D573
 40
@Treatment Temp. 100 °C,
Time 252000 sec
40
@Treatment Temp. 212 °F,
Time 70.0 hour
Hot Air; ASTM D573
 40
@Treatment Temp. 100 °C,
Time 252000 sec
40
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #1; ASTM D471
 40
@Treatment Temp. 100 °C,
Time 252000 sec
40
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #3; ASTM D471
 40
@Treatment Temp. 100 °C,
Time 605000 sec
40
@Treatment Temp. 212 °F,
Time 168 hour
ASTM Oil #1; ASTM D471
 40
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
40
@Treatment Temp. 212 °F,
Time 336 hour
ASTM Oil #3; ASTM D471
 40
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
40
@Treatment Temp. 212 °F,
Time 504 hour
ASTM Oil #3; ASTM D471
 41
@Treatment Temp. 100 °C,
Time 605000 sec
41
@Treatment Temp. 212 °F,
Time 168 hour
ASTM Oil #3; ASTM D471
Tensile Strength at Break 54.5 MPa7900 psiASTM D412
 43.055 MPa
@Time 252000 sec
6244.6 psi
@Time 70.0 hour
Fuel C; ASTM D471
 44.145 MPa
@Time 1.21e+6 sec
6402.7 psi
@Time 336 hour
Fuel C; ASTM D471
 44.69 MPa
@Time 1.81e+6 sec
6482 psi
@Time 504 hour
Fuel C; ASTM D471
 44.69 MPa
@Time 605000 sec
6482 psi
@Time 168 hour
Fuel C; ASTM D471
 54.5 MPa
@Time 1.21e+6 sec
7900 psi
@Time 336 hour
Fuel A; ASTM D471
 57.77 MPa
@Time 605000 sec
8379 psi
@Time 168 hour
Fuel A; ASTM D471
 58.315 MPa
@Time 1.81e+6 sec
8457.9 psi
@Time 504 hour
Fuel A; ASTM D471
 60.045 MPa
@Time 252000 sec
8708.8 psi
@Time 70.0 hour
Fuel A; ASTM D471
 46.87 MPa
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
6798 psi
@Treatment Temp. 212 °F,
Time 504 hour
ASTM Oil #1; ASTM D471
 49.05 MPa
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
7114 psi
@Treatment Temp. 212 °F,
Time 336 hour
ASTM Oil #1; ASTM D471
 55.045 MPa
@Treatment Temp. 100 °C,
Time 605000 sec
7983.6 psi
@Treatment Temp. 212 °F,
Time 168 hour
ASTM Oil #1; ASTM D471
 55.045 MPa
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
7983.6 psi
@Treatment Temp. 212 °F,
Time 504 hour
ASTM Oil #3; ASTM D471
 57.225 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
8299.8 psi
@Treatment Temp. 212 °F,
Time 70.0 hour
Hot Air; ASTM D573
 57.225 MPa
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
8299.8 psi
@Treatment Temp. 212 °F,
Time 504 hour
Hot Air; ASTM D573
 58.86 MPa
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
8537 psi
@Treatment Temp. 212 °F,
Time 336 hour
Hot Air; ASTM D573
 59.405 MPa
@Treatment Temp. 100 °C,
Time 605000 sec
8616.0 psi
@Treatment Temp. 212 °F,
Time 168 hour
Hot Air; ASTM D573
 62.13 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
9011 psi
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #3; ASTM D471
 62.675 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
9090.3 psi
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #1; ASTM D471
 64.31 MPa
@Treatment Temp. 100 °C,
Time 605000 sec
9327 psi
@Treatment Temp. 212 °F,
Time 168 hour
ASTM Oil #3; ASTM D471
 65.4 MPa
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
9490 psi
@Treatment Temp. 212 °F,
Time 336 hour
ASTM Oil #3; ASTM D471
Tensile Stress at Strain  7.60 MPa
@Strain 50 %
1100 psi
@Strain 50 %
ASTM D412
 9.00 MPa
@Strain 100 %
1310 psi
@Strain 100 %
ASTM D412
 20.7 MPa
@Strain 300 %
3000 psi
@Strain 300 %
ASTM D412
 8.73 MPa
@Strain 100 %,
Temperature 100 °C
1270 psi
@Strain 100 %,
Temperature 212 °F
ASTM Oil #1, 336; ASTM D471
 8.82 MPa
@Strain 100 %,
Temperature 100 °C
1280 psi
@Strain 100 %,
Temperature 212 °F
ASTM Oil #1, 70; ASTM D471
 8.91 MPa
@Strain 100 %,
Temperature 100 °C
1290 psi
@Strain 100 %,
Temperature 212 °F
ASTM Oil #1, 168; ASTM D471
 9.00 MPa
@Strain 100 %,
Temperature 100 °C
1310 psi
@Strain 100 %,
Temperature 212 °F
ASTM Oil #1, 50; ASTM D471
 9.18 MPa
@Strain 100 %,
Temperature 100 °C
1330 psi
@Strain 100 %,
Temperature 212 °F
Hot Air, 504; ASTM D573
 9.18 MPa
@Strain 100 %,
Temperature 100 °C
1330 psi
@Strain 100 %,
Temperature 212 °F
ASTM Oil #3, 70; ASTM D471
 9.18 MPa
@Strain 100 %,
Temperature 100 °C
1330 psi
@Strain 100 %,
Temperature 212 °F
ASTM Oil #3, 504; ASTM D471
 9.27 MPa
@Strain 100 %,
Temperature 100 °C
1340 psi
@Strain 100 %,
Temperature 212 °F
Hot Air, 168; ASTM D573
 9.27 MPa
@Strain 100 %,
Temperature 100 °C
1340 psi
@Strain 100 %,
Temperature 212 °F
Hot Air, 336; ASTM D573
 9.27 MPa
@Strain 100 %,
Temperature 100 °C
1340 psi
@Strain 100 %,
Temperature 212 °F
ASTM Oil #3, 168; ASTM D471
 9.36 MPa
@Strain 100 %,
Temperature 100 °C
1360 psi
@Strain 100 %,
Temperature 212 °F
Hot Air, 70; ASTM D573
 9.36 MPa
@Strain 100 %,
Temperature 100 °C
1360 psi
@Strain 100 %,
Temperature 212 °F
ASTM Oil #3, 336; ASTM D471
 18.837 MPa
@Strain 300 %,
Temperature 100 °C
2732.1 psi
@Strain 300 %,
Temperature 212 °F
ASTM Oil #1, 50; ASTM D471
 19.665 MPa
@Strain 300 %,
Temperature 100 °C
2852.2 psi
@Strain 300 %,
Temperature 212 °F
ASTM Oil #1, 336; ASTM D471
 19.872 MPa
@Strain 300 %,
Temperature 100 °C
2882.2 psi
@Strain 300 %,
Temperature 212 °F
Hot Air, 336; ASTM D573
 20.286 MPa
@Strain 300 %,
Temperature 100 °C
2942.2 psi
@Strain 300 %,
Temperature 212 °F
ASTM Oil #1, 168; ASTM D471
 20.286 MPa
@Strain 300 %,
Temperature 100 °C
2942.2 psi
@Strain 300 %,
Temperature 212 °F
ASTM Oil #3, 504; ASTM D471
 20.493 MPa
@Strain 300 %,
Temperature 100 °C
2972.3 psi
@Strain 300 %,
Temperature 212 °F
Hot Air, 504; ASTM D573
 20.7 MPa
@Strain 300 %,
Temperature 100 °C
3000 psi
@Strain 300 %,
Temperature 212 °F
Hot Air, 70; ASTM D573
 21.114 MPa
@Strain 300 %,
Temperature 100 °C
3062.3 psi
@Strain 300 %,
Temperature 212 °F
Hot Air, 168; ASTM D573
 21.114 MPa
@Strain 300 %,
Temperature 100 °C
3062.3 psi
@Strain 300 %,
Temperature 212 °F
ASTM Oil #1, 70; ASTM D471
 21.114 MPa
@Strain 300 %,
Temperature 100 °C
3062.3 psi
@Strain 300 %,
Temperature 212 °F
ASTM Oil #3, 336; ASTM D471
 22.77 MPa
@Strain 300 %,
Temperature 100 °C
3303 psi
@Strain 300 %,
Temperature 212 °F
ASTM Oil #3, 168; ASTM D471
 22.977 MPa
@Strain 300 %,
Temperature 100 °C
3332.5 psi
@Strain 300 %,
Temperature 212 °F
ASTM Oil #3, 70; ASTM D471
 7.11 MPa
@Time 252000 sec,
Strain 100 %
1030 psi
@Time 70.0 hour,
Strain 100 %
Fuel C; ASTM D471
 7.56 MPa
@Strain 100 %,
Time 605000 sec
1100 psi
@Strain 100 %,
Time 168 hour
Fuel C; ASTM D471
 7.65 MPa
@Strain 100 %,
Time 1.21e+6 sec
1110 psi
@Strain 100 %,
Time 336 hour
Fuel C; ASTM D471
 7.74 MPa
@Strain 100 %,
Time 1.81e+6 sec
1120 psi
@Strain 100 %,
Time 504 hour
Fuel C; ASTM D471
 8.82 MPa
@Strain 100 %,
Time 605000 sec
1280 psi
@Strain 100 %,
Time 168 hour
Fuel A; ASTM D471
 8.91 MPa
@Strain 100 %,
Time 1.81e+6 sec
1290 psi
@Strain 100 %,
Time 504 hour
Fuel A; ASTM D471
 9.00 MPa
@Strain 100 %,
Time 1.21e+6 sec
1310 psi
@Strain 100 %,
Time 336 hour
Fuel A; ASTM D471
 9.09 MPa
@Time 252000 sec,
Strain 100 %
1320 psi
@Time 70.0 hour,
Strain 100 %
Fuel A; ASTM D471
 13.662 MPa
@Time 252000 sec,
Strain 300 %
1981.5 psi
@Time 70.0 hour,
Strain 300 %
Fuel C; ASTM D471
 14.904 MPa
@Time 605000 sec,
Strain 300 %
2161.6 psi
@Time 168 hour,
Strain 300 %
Fuel C; ASTM D471
 14.904 MPa
@Strain 300 %,
Time 1.81e+6 sec
2161.6 psi
@Strain 300 %,
Time 504 hour
Fuel C; ASTM D471
 15.111 MPa
@Strain 300 %,
Time 1.21e+6 sec
2191.7 psi
@Strain 300 %,
Time 336 hour
Fuel C; ASTM D471
 19.665 MPa
@Time 605000 sec,
Strain 300 %
2852.2 psi
@Time 168 hour,
Strain 300 %
Fuel A; ASTM D471
 20.079 MPa
@Strain 300 %,
Time 1.81e+6 sec
2912.2 psi
@Strain 300 %,
Time 504 hour
Fuel A; ASTM D471
 20.7 MPa
@Strain 300 %,
Time 1.21e+6 sec
3000 psi
@Strain 300 %,
Time 336 hour
Fuel A; ASTM D471
 21.321 MPa
@Time 252000 sec,
Strain 300 %
3092.4 psi
@Time 70.0 hour,
Strain 300 %
Fuel A; ASTM D471
Elongation at Break 500 %500 %ASTM D412
 460 %
@Time 605000 sec
460 %
@Time 168 hour
Fuel C; ASTM D471
 470 %
@Time 605000 sec
470 %
@Time 168 hour
Fuel A; ASTM D471
 475 %
@Time 1.81e+6 sec
475 %
@Time 504 hour
Fuel C; ASTM D471
 480 %
@Time 252000 sec
480 %
@Time 70.0 hour
Fuel A; ASTM D471
 480 %
@Time 1.21e+6 sec
480 %
@Time 336 hour
Fuel C; ASTM D471
 485 %
@Time 1.21e+6 sec
485 %
@Time 336 hour
Fuel A; ASTM D471
 490 %
@Time 1.81e+6 sec
490 %
@Time 504 hour
Fuel A; ASTM D471
 495 %
@Time 252000 sec
495 %
@Time 70.0 hour
Fuel C; ASTM D471
 500 %
@Treatment Temp. 100 °C,
Time 252000 sec
500 %
@Treatment Temp. 212 °F,
Time 70.0 hour
Hot Air; ASTM D573
 510 %
@Treatment Temp. 100 °C,
Time 605000 sec
510 %
@Treatment Temp. 212 °F,
Time 168 hour
Hot Air; ASTM D573
 510 %
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
510 %
@Treatment Temp. 212 °F,
Time 336 hour
Hot Air; ASTM D573
 515 %
@Treatment Temp. 100 °C,
Time 252000 sec
515 %
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #3; ASTM D471
 525 %
@Treatment Temp. 100 °C,
Time 605000 sec
525 %
@Treatment Temp. 212 °F,
Time 168 hour
ASTM Oil #3; ASTM D471
 525 %
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
525 %
@Treatment Temp. 212 °F,
Time 504 hour
Hot Air; ASTM D573
 530 %
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
530 %
@Treatment Temp. 212 °F,
Time 336 hour
ASTM Oil #1; ASTM D471
 540 %
@Treatment Temp. 100 °C,
Time 605000 sec
540 %
@Treatment Temp. 212 °F,
Time 168 hour
ASTM Oil #1; ASTM D471
 550 %
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
550 %
@Treatment Temp. 212 °F,
Time 504 hour
ASTM Oil #3; ASTM D471
 550 %
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
550 %
@Treatment Temp. 212 °F,
Time 336 hour
ASTM Oil #3; ASTM D471
 550 %
@Treatment Temp. 100 °C,
Time 252000 sec
550 %
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #1; ASTM D471
 595 %
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
595 %
@Treatment Temp. 212 °F,
Time 504 hour
ASTM Oil #1; ASTM D471
Flexural Modulus  0.0517 GPa
@Temperature 70.0 °C
7.50 ksi
@Temperature 158 °F
ASTM D790
 0.0689 GPa
@Temperature 23.0 °C
9.99 ksi
@Temperature 73.4 °F
ASTM D790
Compressive Strength 0.700 MPa102 psi2% Deflection; ASTM D 575
 2.10 MPa305 psi5% Deflection; ASTM D 575
 3.90 MPa566 psi10% Deflection; ASTM D 575
 5.50 MPa798 psi15% Deflection; ASTM D 575
 6.90 MPa1000 psi20% Deflection; ASTM D 575
 9.00 MPa1310 psi25% Deflection; ASTM D 575
 23.0 MPa3340 psi50% Deflection; ASTM D 575
Resilience 4545[%], Bayshore; ASTM D2632
Izod Impact, Notched  1.76 J/cm
@Thickness -762 mm
3.30 ft-lb/in
@Thickness -30.0 in
ASTM D256
 NB
@Thickness 584 mm
NB
@Thickness 23.0 in
ASTM D256
Tear Strength 122.6 kN/m699.6 pliDie C; ASTM D624
Taber Abrasion, mg/1000 Cycles 70
@Load 1.00 kg
70
@Load 2.20 lb
[mg] Loss, H-18; ASTM D3489
Compression Set  18 %
@Temperature 23.0 °C,
Time 79200 sec
18 %
@Temperature 73.4 °F,
Time 22.0 hour
as molded; ASTM D395-B
 18 %
@Temperature 23.0 °C,
Time 79200 sec
18 %
@Temperature 73.4 °F,
Time 22.0 hour
postcured; ASTM D395-B
 35 %
@Temperature 100 °C,
Time 79200 sec
35 %
@Temperature 212 °F,
Time 22.0 hour
postcured; ASTM D395-B
 35 %
@Temperature 70.0 °C,
Time 79200 sec
35 %
@Temperature 158 °F,
Time 22.0 hour
postcured; ASTM D395-B
 43 %
@Temperature 70.0 °C,
Time 79200 sec
43 %
@Temperature 158 °F,
Time 22.0 hour
as molded; ASTM D395-B
 60 %
@Temperature 100 °C,
Time 79200 sec
60 %
@Temperature 212 °F,
Time 22.0 hour
as molded; ASTM D395-B
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point 148 °C298 °FRate A; ASTM D1525
Brittleness Temperature >= -67.8 °C>= -90.0 °FASTM D746
Glass Transition Temp, Tg -46.0 °C-50.8 °F
UL RTI, Electrical 50.0 °C
@Thickness 1.50 mm
122 °F
@Thickness 0.0591 in
UL 746B
UL RTI, Mechanical with Impact 50.0 °C
@Thickness 1.50 mm
122 °F
@Thickness 0.0591 in
UL 746B
UL RTI, Mechanical without Impact 50.0 °C
@Thickness 1.50 mm
122 °F
@Thickness 0.0591 in
UL 746B
Flammability, UL94 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 193 - 204 °C379 - 399 °F
Middle Barrel Temperature 193 - 204 °C379 - 399 °F
Front Barrel Temperature 199 - 210 °C390 - 410 °F
Nozzle Temperature 204 - 210 °C399 - 410 °F
Melt Temperature 204 - 216 °C399 - 421 °F
Mold Temperature 15.0 - 40.0 °C59.0 - 104 °F
Injection Pressure 41.4 - 103 MPa6000 - 15000 psi
Back Pressure <= 1.38 MPa<= 200 psi
Cushion <= 0.317 cm<= 0.125 in
 
Compliance PropertiesMetricEnglishComments
FDA YesYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AdvanSource Biomaterials ChronoFlex® AL 55D Biodurable Medical Grade Polyurethane
A. Schulman POLYPUR™ FPU 1156 Thermoplastic Polyurethane
Covestro Desmopan® DP 8785 A Polyurethane
Covestro Desmopan® 6064A TPU
Covestro Desmopan® 3055D Polyurethane

PCOVEST0974a / 238178

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.